A method for swaging a high-density, large-diameter-reduction, multi-layer armored thermocouple

By calculating the number of forging passes and designing the parameters of the forging machine, the problem of complex forging processes for armored wire products in high vibration and high temperature environments was solved. This enabled qualified forging of high-density, large-diameter-reduction, multi-layer armored thermocouples, improving process reliability and product performance.

CN117483602BActive Publication Date: 2026-11-24TIANJING AVIATION ELECTRO-MECHANICAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311526341.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-15
Publication Date
2026-11-24
Estimated Expiration
2043-11-15

AI Technical Summary

Technical Problem

The existing rotary forging process for armored wire products has problems such as complex process, insufficient product strength and insulation, making it difficult to apply in complex environments with high vibration and high temperature, which limits the development progress of engines.

Method used

The rotary forging method employs high-density, large-diameter-reduction, multi-layer armored thermocouples. By calculating the number of rotary forging passes and designing rotary forging machine parameters, it ensures that the products are qualified for rotary forging and stably produced in batches under high vibration and high temperature environments. This includes the rotary forging rules for equal diameter and variable diameter products, as well as the corresponding feed speed and holding time.

Benefits of technology

It has achieved qualified rotary forging of high-density, large-diameter-reduction, multi-layer armored thermocouples, reducing design difficulty and improving process reliability. It is suitable for high-vibration and high-temperature complex environments and meets the requirements of high density and large diameter reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117483602B_ABST
    Figure CN117483602B_ABST
Patent Text Reader

Abstract

This invention relates to a rotary forging method for high-density, large-diameter-reduction, multi-layered armored thermocouples, belonging to the field of metal pressure processing technology. The rotary forging method includes: calculating the number of rotary forging passes for the armored thermocouple and designing the rotary forging machine parameters for the armored thermocouple based on the outer diameter of the product and the product's diameter change trend.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a rotary forging method for high-density, large-diameter, multi-layer armored thermocouples, belonging to the field of metal pressure processing technology. Background Technology

[0002] With the development of aircraft engine technology in my country, the demand for sensors with functions such as temperature measurement, high-temperature signal transmission, and overheat detection is increasing. Consequently, the design of armored products is becoming more complex, and their manufacturing processes are becoming more challenging. In particular, the crucial rotary forging process determines both product performance and cost.

[0003] Currently, there are two main forming processes for armored wire products. One is drawing, which is characterized by a simple process method and easy exploration of limiting parameters. However, the outer wall strength and insulation layer density of the product are significantly reduced, making it unable to cope with high vibration and high temperature complex environments. This limits the types of machines that can be used and restricts the development progress of engines. The other is rotary forging, which is characterized by high product strength and good insulation. However, the process method is complex and requires exploration of process parameters.

[0004] In conclusion, a simple and reliable rotary forging process design method needs to be developed for the molding process of armored products. Summary of the Invention

[0005] The purpose of this invention is to enable high-density, large-diameter, multi-layer armored thermocouples to be applied in complex environments with high vibration and high temperature, achieving qualified rotary forging and stable batch production.

[0006] The objective of this invention can be achieved through the following technical solutions:

[0007] This invention provides a rotary forging method for high-density, large-diameter-reduction, multi-layer armored thermocouples, comprising:

[0008] Based on the product's outer diameter and diameter variation trend, calculate the number of forging passes for armored thermocouples and design the parameters of the armored thermocouple forging machine.

[0009] For products with constant diameter, the number of forging passes for the armored thermocouple is calculated based on the product's outer diameter and diameter variation trend, including:

[0010] Based on the product's outer diameter range, the pattern is as follows: φ16~φ10, each forging amount is 2mm; φ10~φ6, each forging amount is 1.5mm; φ6~φ3, each forging amount is 1mm; φ3~φ2, each forging amount is 0.5mm; and φ2~φ1, each forging amount is 0.2mm.

[0011] Based on the equal-diameter rotary forging rule, the actual number of equal-diameter rotary forging passes and the rotary forging amount of each pass can be calculated.

[0012] For products with changing diameters, the number of forging passes for the armored thermocouple is calculated based on the product's outer diameter and the trend of diameter change, including:

[0013] Based on the product shape segment range, the rule is that the first variable diameter rotary forging is the transition cone segment, and the second variable diameter rotary forging is the small diameter segment. If the length of the small diameter segment is greater than 10 times the diameter, the second variable diameter rotary forging needs to be divided into several equal parts, and the length of each rotary forging should not be greater than 10 times the diameter. The segmentation requirement for the product shape segment is to ensure that the inner and outer shapes of the same segment are continuous, monotonous and smooth, without inflection points and distortion points.

[0014] Based on the variable diameter rotary forging rules, the actual number of variable diameter rotary forging passes and the rotary forging amount for each pass can be calculated.

[0015] For products with both diameter and diameter variations, the number of forging passes for the armored thermocouple is calculated based on the product's outer diameter and the diameter variation trend, including:

[0016] The sum of the number of forging passes for equal diameter and the number of forging passes for variable diameter is taken as the number of forging passes for armored thermocouples.

[0017] For products of constant diameter, the design parameters for the armored thermocouple rotary forging machine include:

[0018] Machine tool parameters are divided according to the range of product outer diameter dimensions. The rules are as follows: for φ16~φ10, the minimum feed rate is 5mm / s; for φ10~φ6, the minimum feed rate is 3mm / s; for φ6~φ3, the minimum feed rate is 1mm / s; for φ3~φ2, the minimum feed rate is 0.5mm / s; and for φ2~φ1, the minimum feed rate is 0.2mm / s.

[0019] For products with variable diameters, the design parameters for the armored thermocouple rotary forging machine include:

[0020] First, the parameters of the variable diameter rotary forging machine are divided according to the product shape range. Then, the parameters of the variable diameter rotary forging machine are divided according to the product diameter reduction, that is, the difference between the outer diameter before and after rotary forging.

[0021] The parameters of variable diameter rotary forging machine tools are divided according to the product shape range, including:

[0022] For the transition cone section, the diameter reduction must be less than 50%.

[0023] For narrow diameter sections, the reduction in diameter must be greater than 50%.

[0024] The parameters of variable diameter rotary forging machine tools are defined based on the product's diameter reduction, i.e., the difference between the outer diameter before and after rotary forging. These parameters include:

[0025] For the transition cone section, when the diameter reduction is greater than 50%, the feed rate is a minimum of 0.5 mm / s and the holding time is a minimum of 1.5 s;

[0026] For small diameter sections, when the diameter reduction is less than 50%, the feed rate is a minimum of 0.75 mm / s and the holding time is a minimum of 2 seconds; when the diameter reduction is greater than 50%, the feed rate is a minimum of 0.5 mm / s and the holding time is a minimum of 3 seconds.

[0027] The purpose of this invention is to achieve the following beneficial effects:

[0028] This invention relates to a rotary forging method for high-density, large-diameter-reduction, multi-layer armored thermocouples. This method is simple, reliable, has clear rules and distinct boundaries, and enables qualified rotary forging and stable batch production of high-density, large-diameter-reduction, multi-layer armored thermocouples applied in complex environments with high vibration and high temperature. It reduces the difficulty of product design and improves process reliability. Attached Figure Description

[0029] Figure 1 This is a schematic diagram of the cross-section of an armored thermocouple.

[0030] Figure 2 This is a schematic diagram of a variable diameter rotary forging of an armored thermocouple. Detailed Implementation

[0031] The objective of this invention can be achieved through the following technical solutions:

[0032] This invention provides a rotary forging method for high-density, large-diameter-reduction, multi-layered armored thermocouples. The method consists of two parts: a design method for the number of rotary forging passes and a design method for the rotary forging machine parameters. Taking the product shape and dimensions as input, the output is the number of rotary forging passes; taking both the product shape and dimensions and the number of rotary forging passes as input, the output is the rotary forging machine parameters. Only by calculating the correct number of rotary forging passes and the corresponding rotary forging machine parameters can the rotary forging of high-density, large-diameter-reduction, multi-layered armored thermocouples be successfully completed.

[0033] The present invention will now be described in detail with reference to specific embodiments.

[0034] 1) Calculation method for the number of forging passes of armored thermocouples

[0035] The number of forging passes for armored thermocouples is equal to the sum of the number of forging passes with constant diameter and the number of forging passes with variable diameter. There is a significant difference in the calculation of the number of forging passes with constant diameter and the number of forging passes with variable diameter.

[0036] Equal-diameter rotary forging is categorized based on the product's outer diameter range. The general rule is as follows: φ16~φ10, each forging pass is 2mm; φ10~φ6, each forging pass is 1.5mm; φ6~φ3, each forging pass is 1mm; φ3~φ2, each forging pass is 0.5mm; and φ2~φ1, each forging pass is 0.2mm. Based on this rule, the required number of equal-diameter rotary forging passes and the forging amount per pass can be calculated.

[0037] While it is possible to obtain qualified products by forging with a higher forging amount per pass, it may result in defects such as cracking of the outer wall and increased roundness of the outer diameter, leading to product rework or scrap.

[0038] Variable diameter rotary forging is divided according to the product shape range. The rule is that the first variable diameter rotary forging is the transition cone section, and the second variable diameter rotary forging is the smaller diameter section. If the length of the smaller diameter section is greater than 10 times the diameter, the second variable diameter rotary forging needs to be divided into several equal parts, with each forging length not exceeding 10 times the diameter. Based on the variable diameter rotary forging rule, the actual number of variable diameter rotary forging passes and the forging amount per pass can be calculated.

[0039] Direct rotary forging can also produce qualified products, but it may produce defects such as cracks on the outer wall of the product and bulging of the insulation layer on the outer wall, leading to product scrap.

[0040] 2) Parameter Design Method for Armored Thermocouple Rotary Forging Machine

[0041] The machine tool parameters for equal-diameter rotary forging are also divided according to the product's outer diameter range. The general rule is as follows: for φ16~φ10, the minimum feed rate is 5mm / s; for φ10~φ6, the minimum feed rate is 3mm / s; for φ6~φ3, the minimum feed rate is 1mm / s; for φ3~φ2, the minimum feed rate is 0.5mm / s; and for φ2~φ1, the minimum feed rate is 0.2mm / s.

[0042] While it is possible to obtain qualified products by rotating forging at a feed rate higher than the minimum, defects such as cracking of the outer wall and bulging of the insulation layer may occur, leading to product scrap.

[0043] The machine tool parameters for variable diameter rotary forging are first divided by the range of the product shape segment, and then by the reduction in diameter, resulting in four types. The rules are as follows: For the transition tapered segment rotary forging, if the reduction in diameter is less than 50%, the minimum feed rate is 1 mm / s and the minimum holding time is 1 second; for the transition tapered segment rotary forging, if the reduction in diameter is greater than 50%, the minimum feed rate is 0.5 mm / s and the minimum holding time is 1.5 seconds; for the small diameter segment rotary forging, if the reduction in diameter is less than 50%, the minimum feed rate is 0.75 mm / s and the minimum holding time is 2 seconds; for the small diameter segment rotary forging, if the reduction in diameter is greater than 50%, the minimum feed rate is 0.5 mm / s and the minimum holding time is 3 seconds.

[0044] Rotary forging at a feed rate higher than the minimum can also produce qualified products, but it may result in defects such as cracking of the outer wall of the product or bulging of the insulation layer on the outer wall, leading to product scrap. Rotary forging at a holding time higher than the minimum can also produce qualified products, but it may result in spiral patterns on the outer wall of the product or direct cracking, leading to product rework or scrap.

[0045] 3) Design method for armored thermocouple rotary forging process

[0046] First, the forging passes are decomposed based on the structure and dimensions of the armored thermocouple, and then the forging passes are calculated using the method for calculating the forging passes of armored thermocouples. If the external dimensions of the armored thermocouple are uniform and consistent, the equal-diameter forging pass calculation method is used; if the external dimensions of the armored thermocouple exhibit stepped changes, the equal-diameter forging plus variable-diameter forging pass calculation method is used.

[0047] Then, based on the calculation results of each pass, the machine tool parameters are designed using the armored thermocouple rotary forging machine parameter design method. The feed rate and holding time of the machine tool are determined according to the dimensions of each rotary forging pass.

[0048] Finally, the forging passes and corresponding machine tool parameters were integrated into a forging process. Trial forging was conducted using this process, and the machine tool parameters were fine-tuned based on the results to complete the design of the forging process for armored thermocouples.

[0049] This invention relates to a rotary forging method for high-density, large-diameter-reduction, multi-layer armored thermocouples, which can simultaneously meet the requirements of 2500 mg / cm³. 3 The above-mentioned compacted density and diameter reduction of over 60% three-layer armored thermocouples were successfully rotary forged. This rotary forging method includes methods for designing the number of rotary forging passes and the parameters of the rotary forging machine. The method relies solely on the rotary forging die and machine tool, without manual intervention, thus ensuring high reliability. This invention realizes a rotary forging method for high-density, large-diameter-reduction, multi-layer armored thermocouples, reducing design difficulty and improving process reliability.

Claims

1. A rotary forging method for a high-density, large-diameter-reduction, multi-layer armored thermocouple, characterized in that, include: Based on the product's outer diameter and diameter variation trend, calculate the number of forging passes for the armored thermocouple. Design parameters for armored thermocouple rotary forging machine tool; For products with constant diameter, the number of forging passes for the armored thermocouple is calculated based on the product's outer diameter and diameter variation trend, including: Based on the product's outer diameter range, the pattern is as follows: φ16~φ10, each forging amount is 2mm; φ10~φ6, each forging amount is 1.5mm; φ6~φ3, each forging amount is 1mm; φ3~φ2, each forging amount is 0.5mm; and φ2~φ1, each forging amount is 0.2mm. According to the equal-diameter rotary forging law, the actual number of equal-diameter rotary forging passes and the rotary forging amount of each pass can be calculated. For products with changing diameters, the number of forging passes for the armored thermocouple is calculated based on the product's outer diameter and the trend of diameter change, including: Based on the product shape segment range, the rule is that the first variable diameter rotary forging is the transition cone segment, and the second variable diameter rotary forging is the small diameter segment. If the length of the small diameter segment is greater than 10 times the diameter, the second variable diameter rotary forging needs to be divided into several equal parts, and the length of each rotary forging should not be greater than 10 times the diameter. The segmentation requirement for the product shape segment is to ensure that the inner and outer shapes of the same segment are continuous, monotonous and smooth, without inflection points and distortion points. According to the variable diameter rotary forging law, the actual number of variable diameter rotary forging passes and the rotary forging amount of each variable diameter rotary forging pass can be calculated. For products of constant diameter, the design parameters for the armored thermocouple rotary forging machine include: Machine tool parameters are divided according to the product's outer diameter range. The rules are as follows: for φ16~φ10, the minimum feed rate is 5mm / s; for φ10~φ6, the minimum feed rate is 3mm / s; for φ6~φ3, the minimum feed rate is 1mm / s; for φ3~φ2, the minimum feed rate is 0.5mm / s; and for φ2~φ1, the minimum feed rate is 0.2mm / s. For products with variable diameters, the design parameters for the armored thermocouple rotary forging machine include: First, the parameters of the variable diameter rotary forging machine are divided according to the product shape range. Then, the parameters of the variable diameter rotary forging machine are divided according to the product diameter reduction, that is, the difference between the outer diameter before and after rotary forging.

2. The rotary forging method according to claim 1, characterized in that, For products that simultaneously exhibit both constant and variable diameter characteristics, the number of forging passes for the armored thermocouple is calculated based on the product's outer diameter and the trend of diameter variation, including: The sum of the number of forging passes for equal diameter and the number of forging passes for variable diameter is taken as the number of forging passes for armored thermocouples.

3. The rotary forging method according to claim 2, characterized in that, The machine tool parameters corresponding to variable diameter rotary forging are first divided according to the range of product shape segments, and then according to the product diameter reduction, resulting in four types. The rules are as follows: for the transition cone section rotary forging, if the diameter reduction is less than 50%, the feed rate should be at least 1 mm / s and the holding time should be at least 1 s; for the transition cone section rotary forging, if the diameter reduction is greater than 50%, the feed rate should be at least 0.5 mm / s and the holding time should be at least 1.5 s; for the small diameter section rotary forging, if the diameter reduction is less than 50%, the feed rate should be at least 0.75 mm / s and the holding time should be at least 2 s; for the small diameter section rotary forging, if the diameter reduction is greater than 50%, the feed rate should be at least 0.5 mm / s and the holding time should be at least 3 s.

Citation Information

Patent Citations

  • W10Re-W26Re tungsten-rhenium thermoelectric couple material and preparation method thereof

    CN102130288A

  • Heterogeneous aluminum-magnesium alloy bar and preparation method thereof