Process for the preparation of flaky silver, flaky silver and applications

By controlling the growth of silver crystal surfaces through the microemulsion method, flake silver powder can be directly prepared, solving the problems of time and energy consumption in the existing technology. This achieves efficient and low-cost production of flake silver powder, which is suitable for thick film circuits and thin film switches.

CN117483780BActive Publication Date: 2026-11-20SHENZHEN HASHEN TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311649130.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-01
Publication Date
2026-11-20
Estimated Expiration
2043-12-01

AI Technical Summary

Technical Problem

Existing technologies are difficult to efficiently prepare flake silver powder, and the preparation process is time-consuming, energy-intensive, and wasteful. Traditional methods require grinding spherical silver powder into flakes, which wastes raw materials.

Method used

By using the microemulsion method, a reducing agent and a silver salt solution or microemulsion react at the oil-water interface to control the growth direction of silver crystals and directly prepare sheet-like silver, avoiding further processing.

Benefits of technology

It improves production efficiency, reduces production costs, and produces flake silver powder with a diameter-to-thickness ratio of 5-1000, making it suitable for thick-film circuits and membrane switches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117483780B_ABST
    Figure CN117483780B_ABST
Patent Text Reader

Abstract

The application provides a preparation method of flaky silver, flaky silver and application, and particularly relates to the technical field of metal powder preparation. The preparation method of flaky silver is that a reducing agent solution or a reducing agent microemulsion is added into a silver salt solution or a silver salt microemulsion to react, so that the flaky silver is obtained. At least one of the reducing agent and the silver salt is in the form of a microemulsion. The preparation method of flaky silver provided by the application uses a microemulsion to make silver crystal faces grow in a two-dimensional direction, and directly prepares flaky silver in a liquid phase reduction process, so that further processing is avoided, process steps are reduced, production efficiency is improved, and production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal powder preparation technology, and in particular to a method for preparing flake silver, flake silver, and its applications. Background Technology

[0002] Silver is an important industrial production material. The vast majority of applications utilize micro / nano silver powder particles to create silver pastes, which are widely used in various fields including photovoltaics, thick-film circuits, and biomedicine. Based on particle size, silver powder can be classified into fine silver powder (average particle size 10-40 μm), ultrafine silver powder (average particle size 0.5-10 μm), superfine silver powder (average particle size 0.1-0.5 μm), and nano silver powder (average particle size less than 0.1 μm). Based on morphology, it can also be classified into flake-shaped silver powder, spherical silver powder, and dendritic silver powder. Different particle sizes and morphologies of micro / nano silver powder have their relatively suitable application areas. For example, in photovoltaic applications, spherical silver powder is primarily used in photovoltaic positive silver, while flake-shaped silver powder is mainly used in silver pastes for thick-film circuits and thin-film switches.

[0003] The main methods for preparing silver powder include evaporation and condensation, liquid-phase reduction, and silver salt decomposition. Among these, the liquid-phase reduction method is the primary method used for large-scale industrial applications. This method typically uses silver salts such as silver nitrate or silver sulfate as oxidants and vitamin C, formaldehyde, or hydrazine hydrate as reducing agents. A suitable dispersant is then used to control the particle size and morphology, and the redox reaction takes place in an aqueous or organic phase to obtain silver powder. However, in conventional wet reduction methods, the resulting silver powder is generally spherical or near-spherical. Flake-shaped silver powder, which has a wide range of applications, is generally difficult to prepare directly using wet reduction and must be obtained by grinding spherical silver powder using a nano-mill or ball mill. This method of preparing flake powder is relatively time-consuming, energy-intensive, and wastes raw materials.

[0004] In view of this, the present invention is hereby proposed. Summary of the Invention

[0005] One of the objectives of this invention is to provide a method for preparing flake silver, which aims to solve the technical problems of existing flake silver preparation processes having many steps, being time-consuming and energy-intensive, and having large losses during the preparation process.

[0006] The second objective of this invention is to provide a sheet-like silver.

[0007] The third objective of this invention is to provide an application of sheet silver in the fabrication of thick-film circuits or thin-film switches.

[0008] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0009] The first aspect of the present invention provides a method for preparing flake silver, wherein a reducing agent solution or a reducing agent microemulsion is added to a silver salt solution or a silver salt microemulsion to react and obtain the flake silver;

[0010] The reducing agent microemulsion is prepared by adding a hydrophilic emulsifier and a lipophilic emulsifier to a reducing agent solution in any order and dispersing them evenly to obtain the reducing agent microemulsion.

[0011] or,

[0012] The reducing agent microemulsion is prepared by adding a hydrophilic emulsion and a lipophilic emulsifier to a container in any order and dispersing them evenly, and then adding a reducing agent solution to obtain the reducing agent microemulsion.

[0013] The silver salt microemulsion is prepared by adding a hydrophilic emulsifier and a lipophilic emulsifier to a silver salt solution in any order and dispersing them evenly to obtain the silver salt microemulsion.

[0014] or,

[0015] The silver salt microemulsion is prepared by adding a hydrophilic emulsifier and a lipophilic emulsifier to a container in any order and dispersing them evenly, and then adding a silver salt solution to obtain the silver salt microemulsion.

[0016] Among them, at least one of the reducing agent and silver salt is in the form of a microemulsion.

[0017] Furthermore, in the reducing agent microemulsion and / or silver salt microemulsion, the mass ratio of lipophilic emulsifier to hydrophilic emulsifier is 0.3-3.

[0018] Furthermore, the silver salt in the silver salt solution is a soluble silver salt.

[0019] Preferably, the soluble silver salt includes at least one of silver nitrate, sulfate, silver fluoride, silver chlorate, silver acetate, and silver citrate.

[0020] Preferably, the concentration of the silver salt solution is 20 g / L to 320 g / L.

[0021] Furthermore, the reducing agent in the reducing agent solution includes at least one of formaldehyde, hydrazine hydrate, ascorbic acid, and isoascorbic acid.

[0022] Preferably, the concentration of the reducing agent solution is 50 g / L to 200 g / L.

[0023] Furthermore, the hydrophilic emulsifier includes at least one of sodium dodecyl sulfate, sodium octyl polyoxyethylene ether sulfate, polysorbate, octyl polyoxyethylene ether, polyethylene glycol p-isooctylphenyl ether, and nonylphenol polyoxyethylene ether.

[0024] Preferably, in the reducing agent microemulsion and / or silver salt microemulsion, the concentration of the hydrophilic emulsifier is 5 g / L-100 g / L.

[0025] Furthermore, the lipophilic emulsifier includes at least one of cetyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, octanol polyoxyethylene ether, sorbitan fatty acid ester, and oleic acid.

[0026] Preferably, in the reducing agent microemulsion and / or silver salt microemulsion, the concentration of the lipophilic emulsifier is 5 g / L-100 g / L.

[0027] Furthermore, it also includes the washing, filtering, and drying processes after the reaction.

[0028] Preferably, the cleaning process ends when the conductivity of the washing liquid is ≤100μS / cm.

[0029] A second aspect of the present invention provides flake silver prepared by the aforementioned preparation method.

[0030] Furthermore, the diameter-to-thickness ratio is 5-1000.

[0031] A third aspect of the invention provides the application of the aforementioned sheet silver in the fabrication of thick-film circuits or thin-film switches.

[0032] Compared with the prior art, the present invention has at least the following beneficial effects:

[0033] The method for preparing flake silver provided by this invention uses microemulsion to grow silver crystals in a two-dimensional direction, and directly prepares flake silver during liquid-phase reduction, avoiding further processing, reducing process steps, improving production efficiency, and reducing production costs.

[0034] The sheet-like silver provided by this invention has a sheet-like structure with a diameter-to-thickness ratio of 5-1000, which can better meet different application needs.

[0035] The application of sheet silver provided by this invention in the fabrication of thick-film circuits or thin-film switches, given the advantages of sheet silver, is beneficial for the fabrication of thick-film circuits or thin-film switches with better performance, and is conducive to the development of downstream industries. Attached Figure Description

[0036] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0037] Figure 1 Here is a SEM image of the flake silver obtained in Example 1;

[0038] Figure 2 Here is a SEM image of the flake silver obtained in Example 2;

[0039] Figure 3 Here is a SEM image of the flake silver obtained in Example 3;

[0040] Figure 4 Here is a SEM image of the flake silver obtained in Example 4;

[0041] Figure 5 SEM images of the near-spherical silver powder obtained in Comparative Example 1;

[0042] Figure 6 SEM images of the flake-like silver powder obtained in Comparative Example 2;

[0043] Figure 7 SEM images of the silver powder obtained in Comparative Example 3;

[0044] Figure 8 SEM images of the silver powder obtained in Comparative Example 4;

[0045] Figure 9 This is a SEM image of the silver powder obtained in Comparative Example 5. Detailed Implementation

[0046] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The components of the embodiments of the present invention described and shown herein can generally be arranged and designed in various different configurations.

[0047] The first aspect of the present invention provides a method for preparing flake silver, wherein a reducing agent solution or a reducing agent microemulsion is added to a silver salt solution or a silver salt microemulsion to react and obtain the flake silver;

[0048] The reducing agent microemulsion is prepared by adding a hydrophilic emulsifier and a lipophilic emulsifier to a reducing agent solution in any order and dispersing them evenly to obtain the reducing agent microemulsion.

[0049] or,

[0050] The reducing agent microemulsion is prepared by adding a hydrophilic emulsifier and a lipophilic emulsifier into a container in any order and dispersing them evenly, and then adding a reducing agent solution to obtain the reducing agent microemulsion.

[0051] The silver salt microemulsion is prepared by adding a hydrophilic emulsifier and a lipophilic emulsifier to a silver salt solution in any order and dispersing them evenly to obtain the silver salt microemulsion.

[0052] or,

[0053] The silver salt microemulsion is prepared by adding a hydrophilic emulsifier and a lipophilic emulsifier to a container in any order and dispersing them evenly, and then adding a silver salt solution to obtain the silver salt microemulsion.

[0054] Among them, at least one of the reducing agent and silver salt is in the form of a microemulsion.

[0055] The method for preparing flake silver provided by this invention uses microemulsion to grow silver crystals in a two-dimensional direction, and directly prepares flake silver during liquid-phase reduction, avoiding further processing, reducing process steps, improving production efficiency, and reducing production costs.

[0056] Hydrophilic or lipophilic emulsifiers inhibit the growth of certain crystal planes of silver during the reaction, enabling it to achieve two-dimensional growth. The microemulsion reaction system results in different distributions of silver salt in the oil and aqueous phases. After the reducing agent reacts with the silver salt, silver particles are generated in the aqueous phase. The silver particles expand along the oil-water phase interface and enter the aqueous phase microparticles to connect and grow. The presence of the oil phase prevents the growth of silver powder in the oil phase, forming flake-like silver.

[0057] It should be noted that the phrase "adding hydrophilic emulsifier and lipophilic emulsifier in any order and dispersing them evenly" in this invention means adding the two emulsifiers separately, but in any order. For example, it can be understood as adding the hydrophilic emulsifier first, then the lipophilic emulsifier; or it can be adding the lipophilic emulsifier first, then the hydrophilic emulsifier. Each emulsifier added needs to be dispersed evenly to ensure a uniform microemulsion state.

[0058] Furthermore, in the reducing agent microemulsion and / or silver salt microemulsion, the mass ratio of lipophilic emulsifier to hydrophilic emulsifier is 0.3-3.

[0059] When the mass ratio of lipophilic emulsifier to hydrophilic emulsifier is less than 0.3, the microemulsion content is low and the morphology of the formed powder tends to be disordered; when the mass ratio of lipophilic emulsifier to hydrophilic emulsifier is greater than 3, the lipophilic droplets in the microemulsion are encapsulated in larger particles, making dispersion more difficult.

[0060] Typical, but not limiting, mass ratios of lipophilic emulsifier to hydrophilic emulsifier can be, for example, 0.3, 0.6, 0.9, 1.2, 1.5, 1.8, 2.1, 2.4, 2.7, or 3.

[0061] Furthermore, the silver salt in the silver salt solution is a soluble silver salt.

[0062] Preferably, the soluble silver salt includes at least one of silver nitrate, sulfate, silver fluoride, silver chlorate, silver acetate, and silver citrate.

[0063] Preferably, the concentration of the silver salt solution is 20 g / L to 320 g / L.

[0064] When the concentration of the silver salt solution is less than 20 g / L, the yield of silver powder per unit volume of solution is too low to be suitable for large-scale industrial production, and it is easy to generate a mixture of flake powder and spherical powder during the microemulsion preparation process; when the concentration of the silver salt solution is greater than 320 g / L, the dispersibility of the produced silver powder is problematic, and the adhesion between powders is very serious.

[0065] Typical, but not limiting, concentrations of silver salt solutions can be any value ranging from 20 g / L to 320 g / L.

[0066] Furthermore, the reducing agent in the reducing agent solution includes at least one of formaldehyde, hydrazine hydrate, ascorbic acid, and isoascorbic acid.

[0067] Preferably, the concentration of the reducing agent solution is 50 g / L to 200 g / L.

[0068] The concentration of the reducing agent corresponds to the concentration of the silver salt. Based on the chemical reaction process, the amount of reducing agent used exceeds the amount of silver salt to ensure a complete reaction, and the concentration of the reducing agent is kept within a suitable range. When the concentration of the reducing agent solution is less than 50 g / L, the solution concentration is too low, resulting in excessive production waste liquid; when the concentration of the reducing agent solution is greater than 200 g / L, the solution concentration is too high, leading to problems with powder dispersion and severe powder adhesion.

[0069] Typical, but not limiting, concentrations of the reducing agent solution may be, for example, 50 g / L, 70 g / L, 90 g / L, 110 g / L, 130 g / L, 150 g / L, or 200 g / L.

[0070] Furthermore, the hydrophilic emulsifier includes at least one of sodium dodecyl sulfate, sodium octyl polyoxyethylene ether sulfate, polysorbate, octyl polyoxyethylene ether, polyethylene glycol p-isooctylphenyl ether, and nonylphenol polyoxyethylene ether.

[0071] Preferably, in the reducing agent microemulsion and / or silver salt microemulsion, the concentration of the hydrophilic emulsifier is 5 g / L-100 g / L.

[0072] When the concentration of the hydrophilic emulsifier is less than 5 g / L, the microemulsion concentration is too low, resulting in a decrease or absence of the ability to shape the powder, and making it easier to form spherical powders. When the concentration of the hydrophilic emulsifier is greater than 100 g / L, the microemulsion loss is relatively large, making it unsuitable for large-scale industrial production.

[0073] Typical, but not limiting, concentrations of hydrophilic emulsifiers can be, for example, 5 g / L, 10 g / L, 30 g / L, 50 g / L, 70 g / L, 90 g / L, or 100 g / L.

[0074] Furthermore, the lipophilic emulsifier includes at least one of cetyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, octanol polyoxyethylene ether, sorbitan fatty acid ester, and oleic acid.

[0075] Preferably, in the reducing agent microemulsion and / or silver salt microemulsion, the concentration of the lipophilic emulsifier is 5 g / L-100 g / L.

[0076] When the concentration of lipophilic emulsifier is less than 5 g / L, its ability to shape powder decreases or is lost, and it is easier to form spherical powder. When the concentration of lipophilic emulsifier is greater than 100 g / L, the loss of microemulsion is large, making it unsuitable for large-scale industrial production and waste liquid treatment difficult.

[0077] Typical, but not limiting, concentrations of lipophilic emulsifiers can be, for example, 5 g / L, 10 g / L, 30 g / L, 50 g / L, 70 g / L, 90 g / L, or 100 g / L.

[0078] Furthermore, it also includes the washing, filtering, and drying processes after the reaction.

[0079] Preferably, the cleaning process ends when the conductivity of the washing liquid is ≤100μS / cm.

[0080] A second aspect of the present invention provides flake silver prepared by the preparation method described above.

[0081] Furthermore, the diameter-to-thickness ratio is 5-1000. Typical but non-limiting diameter-to-thickness ratios are 5, 10, 50, 100, 300, 500, or 1000.

[0082] The sheet-like silver provided by this invention has a sheet-like structure with a diameter-to-thickness ratio of 5-1000, which can better meet different application needs.

[0083] A third aspect of the invention provides the application of the aforementioned sheet silver in the fabrication of thick-film circuits or thin-film switches.

[0084] The application of sheet silver provided by this invention in the fabrication of thick-film circuits or thin-film switches, given the advantages of sheet silver, is beneficial for the fabrication of thick-film circuits or thin-film switches with better performance, and is conducive to the development of downstream industries.

[0085] The following detailed description of some embodiments of the present invention is provided in conjunction with examples. Unless otherwise specified, the following embodiments and features can be combined with each other. Unless otherwise specified, the raw materials used in the present invention are commercially available.

[0086] Example 1

[0087] This embodiment provides a sheet-like silver, the preparation process of which is as follows:

[0088] 1. Take 30g of ascorbic acid and add it to 300g of water. Stir until it is fully dissolved. Then slowly add 15g of oleic acid and stir. Add 5g of Triton X-100 and homogenize with a homogenizer to form a milky white microemulsion.

[0089] 2. Prepare 250 mL of 1 mol / L silver nitrate solution. While stirring, add the milky white ascorbic acid microemulsion obtained in step 1 to the silver nitrate solution to form a gray precipitate. Wash, filter, and dry the gray precipitate to obtain flake silver.

[0090] Example 2

[0091] This embodiment provides a sheet-like silver, the preparation process of which is as follows:

[0092] 1. Add 25g of ascorbic acid to 300g of water and stir until fully dissolved to obtain a reducing agent solution. Add 7.5g of oleic acid and 2.5g of Triton X-100 to the solution and use an ultrasonic cleaner to vibrate until homogeneous, forming a milky white microemulsion.

[0093] 2. Prepare 250 mL of 0.8 mol / L silver nitrate solution, add 7.5 g of oleic acid and 2.5 g of Triton X-100 to it, and use an ultrasonic cleaner to vibrate evenly to form a milky white microemulsion.

[0094] 3. Under electric stirring, the silver nitrate microemulsion obtained in step 2 is added to the ascorbic acid microemulsion obtained in step 1 to form a gray precipitate. The gray precipitate is washed, filtered, and dried to obtain flake silver.

[0095] Example 3

[0096] This embodiment provides a sheet-like silver, the preparation process of which is as follows:

[0097] 1. Take 25g of ascorbic acid and add it to 300g of water. Stir until it is fully dissolved. Then slowly add 5g of Triton X-100 and stir. Add 15g of oleic acid and use an ultrasonic cleaner to vibrate evenly to obtain a milky white reducing agent microemulsion.

[0098] 2. Prepare 250 mL of 0.8 mol / L silver nitrate solution and stir to obtain silver nitrate solution.

[0099] 3. Under electric stirring, the silver nitrate solution obtained in step 2 is added to the ascorbic acid microemulsion to form a gray precipitate. The gray precipitate is washed, filtered, and dried to obtain flake silver.

[0100] Example 4

[0101] This embodiment provides a sheet-like silver, the preparation process of which is as follows:

[0102] 1. Add 25g of ascorbic acid to 300g of water, stir until fully dissolved, and stir until an ascorbic acid solution is formed.

[0103] 2. Prepare 250 mL of 0.8 mol / L silver nitrate solution, then slowly add 5 g of Triton X-100, stir, add 15 g of oleic acid, and use an ultrasonic cleaner to vibrate evenly to obtain a milky white silver nitrate microemulsion.

[0104] 3. Under electric stirring, the ascorbic acid solution obtained in step 1 is added to the silver nitrate microemulsion prepared in step 2 to form a gray-black precipitate. The gray-black precipitate is washed, filtered, and dried to obtain flake silver.

[0105] Comparative Example 1

[0106] This comparative example provides a silver powder, the preparation process of which is as follows:

[0107] 1. Prepare 250 ml of 1 mol / L silver nitrate solution for later use.

[0108] 2. Add 15g of ascorbic acid to 300g of water, stir until dissolved, then slowly add 20g of PVP and dissolve until dissolved to form a pale yellow reducing agent solution.

[0109] 3. Add silver nitrate solution to reducing agent solution under magnetic stirring to form grayish-white precipitate, which is then washed to obtain silver powder particles.

[0110] Comparative Example 2

[0111] This comparative example provides a flake-shaped silver, which is prepared by grinding the silver powder in Comparative Example 1 using a nano-grinding machine: 500g of silver powder, 400g of 0.3-0.4mm diameter zirconium beads, 3kg of alcohol, and 80g of PVP are added, and the mixture is rotated at 2500r / min for 15min in a nano-grinding machine to obtain flake-shaped silver powder.

[0112] Comparative Example 3

[0113] This comparative example provides a silver powder, the preparation process of which is as follows:

[0114] 1. Prepare 250 ml of 0.1 mol / L silver nitrate solution for later use.

[0115] 2. Add 6g of ascorbic acid to 300g of water, stir until dissolved, then slowly add 3g of oleic acid and 0.6g of Triton X-100, and use an ultrasonic cleaner to vibrate until uniform, forming a milky white ascorbic acid microemulsion.

[0116] 3. Silver nitrate solution was slowly added to ascorbic acid microemulsion solution under electric stirring to form a gray precipitate, which was then washed to obtain silver powder particles.

[0117] Comparative Example 4

[0118] This comparative example provides a silver powder, the preparation process of which is similar to that of Example 1. The difference from Example 1 is that Span 80 is used to replace oleic acid and Tween 80 is used to replace Triathon. All other raw materials and steps are the same as those in Example 1.

[0119] 1. Take 30g of ascorbic acid and add it to 300g of water. Stir until it is fully dissolved. Then slowly add 15g of Span 80 and stir. After stirring, add 5g of Tween 80 and stir evenly with a homogenizer to form a milky white microemulsion.

[0120] 2. Prepare 250 mL of 1 mol / L silver nitrate solution. Under stirring, add the milky white ascorbic acid microemulsion obtained in step 1 to the silver nitrate solution to form a gray precipitate. After washing, filtering and drying the grayish white precipitate, obtain spherical silver powder.

[0121] Comparative Example 5

[0122] This comparative example provides a silver powder, the preparation process of which is as follows:

[0123] 1. Prepare 250 ml of 0.4 mol / L silver nitrate solution, then slowly add 8 g of Tween 80. After it is fully dissolved, add another 8 g of Span 80 and use an ultrasonic cleaner to vibrate it evenly to form a milky white silver nitrate microemulsion.

[0124] 2. Take 15g of ascorbic acid and add it to 300g of water. Stir well and dissolve completely. Then slowly add 8g of Tween 80 and dissolve completely. Then add 8g of Span 80 to make silver nitrate microemulsion. Use an ultrasonic cleaner to vibrate evenly to form a milky white ascorbic acid microemulsion.

[0125] 3. Under magnetic stirring, ascorbic acid microemulsion is slowly added to silver nitrate microemulsion solution to form a gray precipitate, which is then washed to obtain silver powder particles.

[0126] Experimental Example 1

[0127] The product dimensions obtained from Examples 1-6 and Comparative Examples 1-3 were measured. The measurement instrument used was a scanning electron microscope to observe the morphology and size of the silver powder particles. The diameter to thickness ratio of the silver powder was calculated using ImageJ measurement software. The data obtained are shown in Table 1 below.

[0128] Table 1 Particle Size Statistics

[0129]

[0130]

[0131] As shown in Table 1, 1. Through Examples 1-4, the microemulsion method can directly obtain flake silver powder based on the wet reduction method, avoiding the cumbersome process of grinding spherical silver powder required in the traditional flake silver production process, thus improving production efficiency and reducing production costs; this method only uses the nonionic surfactant Triton X-100 and the co-surfactant oleic acid, avoiding the use of dispersants and relatively reducing the pressure on wastewater treatment. Whether the reducing agent and silver salt solution are both prepared as microemulsions for reaction, or one reagent is prepared as a microemulsion while the other remains a solution, and the order in which the reducing agent and silver salt are added, will affect the morphology and size of the powder. The relatively optimized flake powder manufacturing process is shown in Example 1, where ascorbic acid microemulsion is added to silver nitrate solution for reaction, which can obtain flake powder with a diameter of approximately 5-15 micrometers and a diameter-to-thickness ratio of approximately 10-200.

[0132] Experimental Example 2

[0133] The silver powders obtained in Examples 1-4 and Comparative Examples 1-5 were subjected to SEM, and the corresponding SEM images are shown below. Figures 1-9 As shown.

[0134] from Figure 1 , Figure 2 , Figure 3 , Figure 4 By changing whether the reaction solution was prepared as a microemulsion and adjusting the order of addition of the reaction solution, flake-like silver with different morphologies and sizes was prepared in Examples 1-4. Figure 5, Figure 6 , Figure 7 , Figure 8 , Figure 9 It can be seen that the preparation methods of Comparative Examples 1-5 yielded silver powder morphology. Figure 5 This demonstrates how, in Comparative Example 1, a conventional liquid-phase reduction method was used with PVP as a dispersant to prepare near-spherical silver powder. Figure 6 The example shown is a lamellar silver powder prepared by ball milling spherical powder, as presented in Comparative Example 2. Figure 7 In Comparative Example 3, a mixture of flake-shaped and spherical silver powder was prepared by reducing the concentration of the reaction solution. Figure 8 In Comparative Example 4, when Tween 80 and Span 80 are used instead of Triathon X100 and oleic acid to prepare microemulsions, under certain reaction solution concentration conditions, flake powder cannot be obtained, but rather spherical powder with an open-pore structure is obtained. Figure 9 In Comparative Example 5, when Tween 80 and Span 80 are used and the concentration of the reaction solution is reduced, spherical silver powder with a diameter of several hundred nanometers can be prepared. This method is also similar to the traditional microemulsion method for preparing nanoparticles.

[0135] In summary, this method can form silver powder products of various morphologies by changing the formulation and feeding method of the microemulsion. In addition to traditional nanoparticles, various morphologies and sizes of flake silver powder were obtained in Examples 1-4. It can be seen that oleic acid or Triton solution inhibits the growth of certain crystal faces during the reaction, enabling two-dimensional growth. During the reaction of the microemulsion, the interfaces of two or more liquids are layered, and the oleic acid has a high viscosity. The growth of silver powder particles proceeds along the liquid interface, eventually forming flake silver powder. Furthermore, the particle size and layer thickness of the obtained flake silver powder can be controlled by changing the concentration of the reaction solution, the addition of the reaction microemulsion, the stirring method and stirring speed, and the dropping reaction method. The effect obtained in Comparative Example 4 is that small crystal particles aggregate into large cauliflower-like crystals with spherical shapes. This growth mode is similar to the general wet reduction silver powder preparation method, but the surfactants and other components play a certain role as dispersants to shape the particles into spherical shapes. During the reaction, the silver nitrate solution rapidly penetrates the droplet environment constructed by the surfactant, resulting in a fast reaction and the formation of large, near-spherical silver powder. Comparative Example 5 yielded silver nanoparticles of several hundred nanometers in size. This situation is consistent with the classic microemulsion preparation method, where both reactants form microemulsions, and the two microemulsion particles collide and react with each other in the solution. The microemulsions create an ideal template and microenvironment, effectively limiting the growth of silver powder grains, thus ultimately producing smaller silver powder particles. These examples demonstrate that this method has morphology control over silver powder growth, especially in directly generating flake-like silver powder in a liquid phase system. Furthermore, the reaction process does not require traditional dispersants such as PVP, reducing the production cost of flake-like silver powder.

[0136] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing flake silver, characterized in that, A reducing agent solution or reducing agent microemulsion is added to a silver salt solution or silver salt microemulsion to react and obtain the flake silver; The reducing agent microemulsion is prepared by adding oleic acid and Triton X-100 to the reducing agent solution in any order and dispersing them evenly to obtain the reducing agent microemulsion. or, The reducing agent microemulsion is prepared by adding oleic acid and Triton X-100 to a container in any order and dispersing them evenly, and then adding the reducing agent solution to obtain the reducing agent microemulsion. The silver salt microemulsion is prepared by adding oleic acid and Triton X-100 to a silver salt solution in any order and dispersing them evenly to obtain the silver salt microemulsion. or, The silver salt microemulsion is prepared by adding oleic acid and Triton X-100 to a container in any order and dispersing them evenly, and then adding a silver salt solution to obtain the silver salt microemulsion. Among them, at least one of the reducing agent and silver salt is in the form of a microemulsion; In the reducing agent microemulsion and / or silver salt microemulsion, the mass ratio of oleic acid to Triton X-100 is 0.3-3; In the reducing agent microemulsion and / or silver salt microemulsion, the concentration of Triton X-100 is 10 g / L-100 g / L, and the concentration of oleic acid is 10 g / L-100 g / L.

2. The preparation method according to claim 1, characterized in that, The silver salt in the silver salt solution is a soluble silver salt.

3. The preparation method according to claim 2, characterized in that, The soluble silver salt includes at least one of silver nitrate, sulfate, silver fluoride, silver chlorate, silver acetate, and silver citrate.

4. The preparation method according to claim 1, characterized in that, The concentration of the silver salt solution is 20 g / L-320 g / L.

5. The preparation method according to claim 1, characterized in that, The reducing agent in the reducing agent solution includes at least one of formaldehyde, hydrazine hydrate, ascorbic acid, and isoascorbic acid.

6. The preparation method according to claim 1, characterized in that, The concentration of the reducing agent solution is 50 g / L-200 g / L.

7. The preparation method according to claim 1, characterized in that, It also includes the washing, filtration and drying processes after the reaction.

8. The preparation method according to claim 7, characterized in that, The cleaning process ends when the conductivity of the washing solution is ≤100μS / cm.

9. A sheet of silver prepared by the preparation method according to any one of claims 1-8.

10. The flake silver according to claim 9, characterized in that, The diameter to thickness ratio is 5-1000.

11. The use of the sheet silver as described in claim 9 or 10 in the fabrication of thick-film circuits or thin-film switches.

Citation Information

Patent Citations

  • Preparation method of micron-sized flake silver powder

    CN116237534A