Nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board and manufacturing method thereof

Through inorganic adhesive bonding technology, dihydrogen phosphate reacts with magnesium oxide to form phosphate-based inorganic adhesive, combining silica aerogel and aluminum silicate fibers to form a nanocrosslinked structure, solving the harmful release of adhesives in artificial boards The problem of insufficient substances and moisture resistance has achieved moisture-proof, fire-proof and high-temperature resistance of multi-layer solid wood boards, and is suitable for high-humidity environments.

CN117484618BActive Publication Date: 2024-11-15FOSHAN OSOLE BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311501279.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-13
Publication Date
2024-11-15
Estimated Expiration
2043-11-13
Patent Text Reader

Abstract

The invention discloses a nano-crosslinked anti-seepage cold-pressed multi-layer solid wood board and a method for making the same, and belongs to the field of building materials. The inorganic glue used includes 35-50 parts of magnesium oxide, 1-5 parts of silica aerogel, 1-2 parts of aluminum silicate fiber, 5-20 parts of dihydrogen phosphate, 5-10 parts of aluminum oxide, and 30-50 parts of water by mass. The present invention does not require any volatile organic compounds, but utilizes dihydrogen phosphate to react with magnesium oxide and aluminum oxide to generate phosphate-based inorganic glue to bond the board, and the inorganic glue is mixed with silica aerogel to improve the high temperature resistance and fire resistance of the board; the phosphate-based inorganic glue can improve the moisture-proof ability of the multi-layer solid wood board, so that the multi-layer solid wood board is not easy to deform; the aluminum silicate fiber can toughen the phosphate-based inorganic glue and improve the fire resistance of the board, and the aluminum silicate fiber is similar to the components in the inorganic glue, and the inorganic glue has good wettability to the aluminum silicate fiber, and the interface bonding force of the two is strong after curing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board and a manufacturing method thereof, and belongs to the field of building materials. Background Art

[0002] Solid wood furniture is expensive. In order to meet the needs of consumers who want cheap but wood-like furniture, artificial boards came into being. Artificial boards are usually made by cutting fast-growing wood into particles, strips or sheets, and then gluing them together with adhesives.

[0003] In the past, the adhesive used in artificial boards (especially wood boards) was urea-formaldehyde glue, which will continuously decompose formaldehyde during long-term use, with a release period of up to ten years. As consumers' knowledge level continues to improve, the harm caused by formaldehyde to human health has attracted more and more attention. Formaldehyde can irritate the eyes, nasal cavity and throat, causing discomfort symptoms such as itchy eyes, tears, and sore throat. Formaldehyde can also irritate the respiratory mucosa, leading to respiratory diseases such as coughing, wheezing, and sputum. People who are exposed to high concentrations of formaldehyde for a long time are also prone to respiratory diseases such as chronic bronchitis and emphysema. Long-term exposure to high concentrations of formaldehyde can cause discomfort symptoms such as redness, itching, and dryness of the skin; formaldehyde can also destroy the natural protective layer of the skin, making the skin sensitive and prone to allergic reactions, such as eczema, dermatitis and other skin diseases. In addition, long-term exposure to high concentrations of formaldehyde can also have a negative impact on the nervous system. Formaldehyde can affect the normal function of the brain, causing headaches, dizziness, and insomnia. The World Health Organization lists formaldehyde as a Class 1 carcinogen. Long-term exposure to a high concentration of formaldehyde will increase the risk of respiratory cancers such as nasopharyngeal cancer, nasal cancer, and laryngeal cancer. Formaldehyde can also cause damage to internal organs such as the thymus, liver, and kidneys, increasing the likelihood of cancer.

[0004] For this reason, in recent years, artificial boards have gradually switched to MDI (diphenylmethane diisocyanate) glue. MDI glue does not release formaldehyde and is resistant to high temperatures. However, MDI still releases benzene air pollutants, and the release period is about one month, which still cannot meet the requirements of immediate installation and living. Although MDI glue is basically non-toxic after a one-month release period, the raw materials for the production of MDI glue are highly toxic, and the protection requirements during production are very high, which undoubtedly increases the production, storage and transportation costs of MDI glue. On the other hand, MDI glue is currently only applicable to particle boards and particle boards, but not to density boards and multi-layer solid wood boards. Therefore, how to make environmentally friendly multi-layer solid wood boards has become a difficult problem that needs to be solved in the field of building materials. Moreover, whether it is urea-formaldehyde glue or MDI glue, although it has a certain water resistance, it is not strong, which makes artificial boards used in high-humidity environments very easy to deform, so places such as bathrooms usually can only use aluminum alloy cabinets. Summary of the invention

[0005] In order to overcome the shortcomings of the prior art, the present invention provides a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board and a manufacturing method thereof. The prepared multi-layer solid wood board does not contain volatile organic matter and has moisture-proof and fire-resistant properties.

[0006] The technical solution adopted by the present invention to solve its technical problem is:

[0007] In a first aspect, the present application provides a method for manufacturing a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board, comprising the following steps:

[0008] Apply inorganic glue on the surface of the veneer;

[0009] stacking a plurality of the single boards and then cold pressing them to obtain a composite board;

[0010] Drying the composite board to obtain the nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board;

[0011] By mass, the inorganic glue includes 35-50 parts of magnesium oxide, 1-5 parts of silica aerogel, 1-2 parts of aluminum silicate fiber, 5-20 parts of dihydrogen phosphate, 5-10 parts of aluminum oxide, and 30-50 parts of water.

[0012] The method for producing a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board provided in the present application does not use any volatile organic compounds, but utilizes the reaction of dihydrogen phosphate and magnesium oxide to generate a phosphate-based inorganic glue to bond the boards, and the inorganic glue is mixed with silica aerogel to improve the high temperature resistance and fire resistance of the boards; although the silica aerogel is hygroscopic, after wrapping it in the phosphate-based inorganic glue, the silica aerogel is hindered from absorbing water, and at the same time, the phosphate-based inorganic glue also enhances the moisture-proof ability of the multi-layer solid wood board, making the multi-layer solid wood board less likely to deform; both the phosphate-based inorganic glue and the silica aerogel are brittle, and the aluminum silicate fiber in the inorganic glue can toughen the phosphate-based inorganic glue, and the aluminum silicate fiber is similar to the component in the inorganic glue of the present application, the inorganic glue has good wettability to the aluminum silicate fiber, and the interface bonding force between the two is strong after curing, and the aluminum silicate fiber can also improve the fire resistance of the board.

[0013] Preferably, the length of the aluminum silicate fiber is 50 μm-100 μm, and the aspect ratio is 10 to 15, which can provide a better toughening effect and improve the bending strength of the plate.

[0014] Furthermore, the dihydrogen phosphate is composed of potassium dihydrogen phosphate and sodium dihydrogen phosphate in a mass ratio of 1:2, and the inorganic glue also contains magnesium chloride. By mass, the inorganic glue includes 45-50 parts of magnesium oxide, 1-5 parts of silica aerogel, 1-2 parts of aluminum silicate fiber, 5-8 parts of dihydrogen phosphate, 5-10 parts of aluminum oxide, 30-50 parts of water, and 1-3 parts of magnesium chloride.

[0015] The dihydrogen phosphate reacts with magnesium oxide to form the main viscous component in the inorganic glue, and aluminum oxide is used as a high-hardness filler. If potassium dihydrogen phosphate is used as all dihydrogen phosphates, the inorganic glue will have high early strength, but it will cure quickly and will be difficult to adapt to the production of multi-layer solid wood boards. Using sodium dihydrogen phosphate as the main dihydrogen phosphate and mixing it with potassium dihydrogen phosphate is conducive to adjusting the curing time of the inorganic glue to adapt to the production rhythm of multi-layer solid wood boards. At the same time, magnesium chloride is added to the components to provide a part of magnesium ions and adjust the pH of the inorganic glue, thereby adjusting the curing speed of the inorganic glue.

[0016] Furthermore, the veneer is pre-treated before being coated with the inorganic glue, and the pre-treatment steps include:

[0017] Soak the veneer in a pretreatment solution;

[0018] draining the veneer;

[0019] By mass, the pretreatment solution includes 20-35 parts of aluminum dihydrogen phosphate, 10-20 parts of magnesium chloride, 0.5-1 part of boric acid, and 30-50 parts of water.

[0020] Pretreatment provides a heated and pressurized acidic environment, which is conducive to removing some lignin and polysaccharides in wood fibers. At the same time, the space originally filled with lignin is filled with aluminum dihydrogen phosphate, magnesium chloride, boric acid and other ingredients. After the inorganic glue is applied, the ions contained in these ingredients can also participate in the reaction of the inorganic glue, which is equivalent to the inorganic glue penetrating into the veneer, making the inorganic glue and the veneer more bonded, and making the board more moisture-proof and mildew-proof after the inorganic glue is cured. The boric acid in the component has a retarding effect, which prevents the large amount of magnesium oxide in the inorganic glue from curing immediately as soon as it contacts the aluminum dihydrogen phosphate on the veneer side. At the same time, magnesium chloride can also provide magnesium ions in the veneer side, which is more conducive to the inorganic glue to penetrate into the veneer before curing.

[0021] Furthermore, the dihydrogen phosphate in the inorganic glue is aluminum dihydrogen phosphate, and the inorganic glue also contains 0.3 parts to 0.5 parts of boric acid.

[0022] Aluminum dihydrogen phosphate can provide acid and phosphate to generate magnesium phosphate-based glue. A small amount of aluminum dihydrogen phosphate can generate aluminum phosphate-based glue as a secondary adhesive component. Aluminum phosphate-based glue is not as brittle as magnesium phosphate-based glue, which can reduce the brittleness of the plate so that the cut is smooth when the plate is cut. In addition to forming magnesium phosphate-based glue, under the action of heating, excess magnesium ions can form -O-Mg-O-bridge chains between aluminum phosphate molecules, making magnesium phosphate-based glue and aluminum phosphate-based glue cross-linked and interpenetrating.

[0023] Furthermore, in the step of drying the composite board, the drying temperature is 90° C.-160° C. and the drying time is 10 h-24 h.

[0024] During the cold pressing process, magnesium phosphate-based glue and aluminum phosphate molecules distributed in the wet magnesium phosphate-based glue are first formed. During the heating required for drying, the aluminum phosphate-based glue also begins to solidify, and the board continues to lose water, thereby forming a cross-linked network of magnesium phosphate-based glue and aluminum phosphate-based glue, thereby improving the toughness of the board.

[0025] Furthermore, the magnesium oxide comprises 5% by mass of light-burned magnesium oxide and 95% by mass of dead-burned magnesium oxide, the particle size distribution of the light-burned magnesium oxide is 15 μm-25 μm, and the particle size distribution of the dead-burned magnesium oxide is 150 μm-250 μm.

[0026] Light-burned magnesium oxide has a fast bonding speed, and light-burned magnesium oxide with small particle size has a faster bonding speed. Heavy-burned magnesium oxide has a slow bonding speed, and heavy-burned magnesium oxide with large particle size has an even slower bonding speed. By mixing low-content light-burned magnesium oxide with small particle size with high-content heavy-burned magnesium oxide with large particle size, the light-burned magnesium oxide with small particle size will first form a skeleton with a certain initial strength, and then the heavy-burned magnesium oxide with large particle size will gradually solidify more slowly, which is conducive to the formation of high-quality magnesium phosphate-based glue, which plays a good bonding and supporting role in the single-board bracket.

[0027] Furthermore, the preparation steps of the inorganic glue include:

[0028] Mixing the light-burned magnesium oxide and the silicon dioxide aerogel to obtain a mixed powder;

[0029] Adding the boric acid and the aluminum dihydrogen phosphate into the water, and then sequentially adding the aluminum silicate fiber, the aluminum oxide and the dead-burned magnesium oxide under stirring at 150 rpm-200 rpm to obtain a mixed solution;

[0030] The stirring speed is increased to 500 rpm-600 rpm, the mixed powder is added to the mixed solution, and stirring is continued for 5 min-10 min to obtain the inorganic glue.

[0031] In the preparation step, a component with a slow setting and activating effect is first added, and then a reinforcing phase and a slowly reacting component are added to obtain a mixed solution with a certain initial viscosity but slow cementation. The lightly calcined magnesium oxide and the silica aerogel are evenly mixed in the mixed powder. After being added to the mixed solution, the lightly calcined magnesium oxide reacts quickly to form a supporting skeleton that wraps or semi-wraps the silica aerogel, which is beneficial to maintaining the hollow state of the silica aerogel and giving full play to the fireproofing and heat-insulating effects of the silica aerogel on the board.

[0032] Furthermore, in the step of soaking the veneer with the pretreatment liquid, the pressure is 100 kPa-150 kPa, the temperature is 100° C.-110° C., and the time is 10 h-20 h, which is beneficial to remove the lignin and polysaccharides on the surface of the veneer as much as possible.

[0033] Furthermore, in the cold pressing step, the pressure acting on the plate is 16 kPa-32 kPa, and the cold pressing time is 6 h-12 h.

[0034] In the second aspect, the present application provides a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board, which is made by the nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board manufacturing method described in the first aspect, and has the advantages of fire resistance, moisture resistance, and no volatile organic compounds.

[0035] The beneficial effects of the present invention are as follows: the present invention does not use any volatile organic matter, but utilizes dihydrogen phosphate to react with magnesium oxide to generate phosphate-based inorganic glue to bond the board material, and the inorganic glue is mixed with silica aerogel to improve the high temperature resistance and fire resistance of the board material; the phosphate-based inorganic glue can improve the moisture resistance of the multi-layer solid wood board, making the multi-layer solid wood board less likely to deform; the aluminum silicate fiber can toughen the phosphate-based inorganic glue and improve the fire resistance of the board material, and the components of the aluminum silicate fiber and the inorganic glue are similar, the inorganic glue has good wettability to the aluminum silicate fiber, and the interface bonding force between the two is strong after curing. DETAILED DESCRIPTION

[0036] It should be understood that, under the premise of no conflict, any and all embodiments of the present invention can be combined with the technical features in any other embodiment or multiple other embodiments to obtain another embodiment. The present invention includes such a combination to obtain another embodiment.

[0037] Unless otherwise specified, all technical and scientific terms used herein have the standard meaning in the field to which the claimed subject matter belongs. If there are multiple definitions for a term, the definition herein shall prevail.

[0038] It should be understood that the singular forms used in the present invention, such as "a", include plural references unless otherwise specified. In addition, the term "comprising" is an open limitation and not a closed form, that is, including the contents specified in the present invention, but not excluding other aspects.

[0039] With the development of material technology, the MDI glue currently used in artificial boards is more environmentally friendly, but there is still a period of pollutant release, and it cannot be installed and lived in immediately. In addition to the disadvantages of poor moisture resistance and inability to be used for multi-layer solid wood boards, MDI glue also has the problem of releasing toxic gases when burned.

[0040] In view of these situations, the embodiment of the present application provides a method for manufacturing a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board, comprising the following steps:

[0041] S1: Apply inorganic glue on the surface of the veneer.

[0042] S2: Multiple single boards are stacked and cold pressed to obtain a composite board.

[0043] S3: Drying the composite board to obtain a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board.

[0044] Among them, the inorganic glue includes 35-50 parts of magnesium oxide, 1-5 parts of silica aerogel, 1-2 parts of aluminum silicate fiber, 5-20 parts of dihydrogen phosphate, 5-10 parts of aluminum oxide, and 30-50 parts of water by mass.

[0045] Those skilled in the art understand that veneer refers to a thin wood board with a thickness of 0.5 mm to 4 mm, obtained by slicing wood. In step S1, the surface of the veneer that needs to be coated with glue is the surface that needs to be bonded. Taking a multi-layer solid wood board consisting of 6 layers of veneer as an example, the 2nd, 3rd, 4th and 5th layers of veneer are coated with glue on both sides; if there is no facing, the 1st layer of veneer is only coated with glue on the bottom surface, and the 6th layer of veneer is only coated with glue on the top surface.

[0046] The method for producing a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board provided in the embodiment of the present application utilizes the reaction of dihydrogen phosphate and magnesium oxide to generate a phosphate-based inorganic glue to bond the boards without using any volatile organic substances.

[0047] Phosphate-based glue itself is non-flammable and moisture-resistant, and the silica aerogel mixed in the inorganic glue can improve the high temperature resistance and fire resistance of the board. The phosphate-based inorganic glue wraps the silica aerogel and can inhibit the water absorption of the silica aerogel, making the multi-layer solid wood board have good moisture resistance and not easy to deform.

[0048] Pure phosphate-based inorganic adhesive is obviously brittle. When cutting a plate bonded by phosphate-based inorganic adhesive, the adhesive layer is prone to collapse, making the cut surface rough. In the embodiment of the present application, aluminum silicate fiber is used to toughen the phosphate-based inorganic adhesive, and the aluminum silicate fiber is similar to the composition of the inorganic adhesive in the present application. The inorganic adhesive has good wettability to the aluminum silicate fiber, and the interface bonding force between the two is strong after curing. At the same time, the aluminum silicate fiber itself is also a refractory material.

[0049] The dihydrogen phosphate can be selected from one or more of ammonium dihydrogen phosphate, sodium dihydrogen phosphate, potassium dihydrogen phosphate, and aluminum dihydrogen phosphate.

[0050] In some embodiments, the dihydrogen phosphate is composed of potassium dihydrogen phosphate and sodium dihydrogen phosphate in a mass ratio of 1:2. The inorganic glue also contains magnesium chloride. By mass, the inorganic glue includes 45-50 parts of magnesium oxide, 1-5 parts of silica aerogel, 1-2 parts of aluminum silicate fiber, 5-8 parts of dihydrogen phosphate, 5-10 parts of aluminum oxide, 30-50 parts of water, and 1-3 parts of magnesium chloride.

[0051] Artificial boards are not moisture-proof because the general adhesives reduce their viscosity, and part of the reason is that wood becomes moldy when it comes into contact with water. The wood used for artificial boards grows much faster than the wood used for log furniture, and the wood is relatively loose. Wood contains cellulose, polysaccharides and lignin. Cellulose is not easy to rot. For example, common paper will not rot even if it is dried in the shade after being wetted by water. The fast-growing wood used for artificial boards contains a higher proportion of lignin and polysaccharides, so it is easy to breed microorganisms and mold.

[0052] Preferably, the veneer is pretreated before being coated with the inorganic adhesive, and the pretreatment steps include:

[0053] S011: Soak the veneer in pretreatment liquid.

[0054] S012: Drain the veneer.

[0055] The pretreatment liquid includes 20-35 parts of aluminum dihydrogen phosphate, 10-20 parts of magnesium chloride, 0.5-1 part of boric acid, and 30-50 parts of water by mass.

[0056] The pretreatment provides an acidic environment of heating and pressurization, which is conducive to removing part of the lignin and polysaccharides on the surface of the veneer. At the same time, the space originally filled with lignin is filled with aluminum dihydrogen phosphate, magnesium chloride, boric acid and other components. After the inorganic glue is applied, the ions contained in these components can also participate in the reaction of the inorganic glue, which is equivalent to the inorganic glue penetrating into the veneer, making the inorganic glue and the veneer more bonded, and making the board more moisture-proof and mildew-proof after the inorganic glue is cured. And because a large amount of lignin and polysaccharides are removed, the nutritional content is greatly reduced for termites, so the multi-layer solid wood board obtained in the embodiment of the present application also has a certain anti-termite effect.

[0057] The boric acid in the pretreatment liquid has a retarding effect, which prevents the large amount of magnesium oxide in the inorganic glue from solidifying immediately upon contacting the aluminum dihydrogen phosphate on the veneer side. At the same time, magnesium chloride can also provide magnesium ions on the veneer side, which is more conducive to the inorganic glue to penetrate deep into the veneer before solidification.

[0058] At the same time, the dihydrogen phosphate in the inorganic glue is also aluminum dihydrogen phosphate, and the inorganic glue also contains 0.3 parts to 0.5 parts of boric acid.

[0059] In addition to providing acidity, aluminum dihydrogen phosphate itself can form aluminum phosphate-based glue as a secondary viscous component. The temperature required for spontaneous curing of aluminum dihydrogen phosphate is relatively high. In the embodiment of the present application, excessive magnesium oxide is added to reduce the curing temperature of aluminum dihydrogen phosphate.

[0060] Specifically, in the step of drying the composite board, the drying temperature is 90° C.-160° C., and the time is 10 h-24 h. While achieving drying and dehumidification, the board can be heated to solidify the aluminum phosphate-based glue.

[0061] Aluminum phosphate-based adhesive is not as brittle as magnesium phosphate-based adhesive, which can reduce the brittleness of the plate so that the cut is smooth when the plate is cut. Magnesium ions can form -O-Mg-O-bridge chains between aluminum phosphate molecules, making the magnesium phosphate-based adhesive and aluminum phosphate-based adhesive cross-linked and interpenetrating, making the plate stronger.

[0062] The main viscous component in the present application is magnesium phosphate-based glue, and the main raw material in the magnesium phosphate-based glue is magnesium oxide. Magnesium oxide is usually obtained by calcining magnesite, and its quality has an important influence on the quality of the glue.

[0063] In some embodiments, the magnesium oxide comprises 5% by mass of light-burned magnesium oxide and 95% by mass of dead-burned magnesium oxide, the particle size distribution of the light-burned magnesium oxide is 15 μm-25 μm, and the particle size distribution of the dead-burned magnesium oxide is 150 μm-250 μm.

[0064] Light-burned magnesium oxide refers to magnesium oxide burned at 800-1000°C, and has a fast gelling speed. The above-mentioned specific particle size needs to be ball-milled in a nitrogen atmosphere to further improve the gelling speed after refinement, and it is conducive to subsequent uniform mixing with silica aerogel. Heavy-burned magnesium oxide refers to magnesium oxide burned at about 1800°C, and has a slow gelling speed. Heavy-burned magnesium oxide with larger particle size has an even slower gelling speed. When light-burned magnesium oxide with a low content and small particle size is mixed with heavy-burned magnesium oxide with a high content and large particle size, the light-burned magnesium oxide with a small particle size will first form a skeleton with a certain initial strength, and then the heavy-burned magnesium oxide with a large particle size will gradually solidify slowly, which is conducive to the formation of high-quality magnesium phosphate-based glue, which plays a good bonding and supporting role in the single-board bracket.

[0065] On this basis, the preparation steps of inorganic glue include:

[0066] S021: Mixing light-burned magnesium oxide and silicon dioxide aerogel to obtain a mixed powder.

[0067] S022: Add boric acid and aluminum dihydrogen phosphate into water, and then add aluminum silicate fiber, aluminum oxide and dead-burned magnesium oxide in sequence under stirring at 150 rpm-200 rpm to obtain a mixed solution.

[0068] S023: Increase the stirring speed to 500rpm-600rpm, add the mixed powder into the mixed solution, and continue stirring for 5min-10min to obtain the inorganic glue.

[0069] Step S022 first adds a component with a slow setting and activation effect, and then adds a reinforcing phase and a slowly reacting component to obtain a mixed solution with a certain initial viscosity but slow cementation. The lightly calcined magnesium oxide and the silica aerogel in the mixed powder are evenly mixed. After being added to the mixed solution, the lightly calcined magnesium oxide reacts quickly to form a supporting skeleton that wraps or semi-wraps the silica aerogel, which is conducive to maintaining the hollow state of the silica aerogel and giving full play to the fireproof and heat-insulating effects of the silica aerogel on the board.

[0070] Example 1

[0071] Inorganic glue is applied on the surface of 2mm thick veneer with a thickness of 0.2mm. The inorganic glue includes 50 parts of magnesium oxide, 5 parts of silica aerogel, 2 parts of aluminum silicate fiber, 8 parts of dihydrogen phosphate, 10 parts of aluminum oxide, 50 parts of water and 1 part of magnesium chloride by mass. The dihydrogen phosphate is composed of potassium dihydrogen phosphate and sodium dihydrogen phosphate in a mass ratio of 1:2.

[0072] The six single boards were stacked and then cold pressed to obtain a composite board. During the cold pressing step, the pressure acting on the board was 32 kPa and the cold pressing time was 10 hours.

[0073] The composite board is dried to obtain a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board at a drying temperature of 110° C. for 24 hours.

[0074] The formaldehyde emission of the board obtained by the test is 0.006mg / m³. The sample was submerged in water and boiled for 10 minutes and then soaked for 6 hours. The static bending strength after soaking was 13.6MPa, and the size of the impact pit was 10.9mm. The fire resistance grade of the dried sample was A2 according to GB8624-2012.

[0075] Example 2

[0076] Soak 2mm thick veneer in pretreatment solution. The pretreatment solution includes 20 parts of aluminum dihydrogen phosphate, 10 parts of magnesium chloride, 1 part of boric acid, and 50 parts of water by mass. Pressurize to 150kPa, temperature to 110℃, and time to 20h.

[0077] Drain the veneer.

[0078] Inorganic glue is applied on the surface of the veneer with a thickness of 0.2 mm. The inorganic glue includes 40 parts of magnesium oxide, 3 parts of silica aerogel, 1 part of aluminum silicate fiber, 20 parts of aluminum dihydrogen phosphate, 5 parts of aluminum oxide, 40 parts of water, and 0.4 parts of boric acid by mass. Among them, magnesium oxide includes 5% of light-burned magnesium oxide and 95% of dead-burned magnesium oxide by mass, and the particle size distribution of light-burned magnesium oxide is 15μm-25μm, and the particle size distribution of dead-burned magnesium oxide is 150μm-250μm.

[0079] The six single boards were stacked and then cold pressed to obtain a composite board. During the cold pressing step, the pressure acting on the board was 30 kPa and the cold pressing time was 12 hours.

[0080] The composite board is dried to obtain a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board at a drying temperature of 160° C. for 20 hours.

[0081] The formaldehyde emission of the board obtained by the test is 0.006mg / m³. The sample was submerged in water and boiled for 10 minutes and then soaked for 6 hours. The static bending strength after soaking was 15.0MPa, and the size of the impact pit was 8.7mm. The fire resistance grade of the dried sample was A2 according to GB8624-2012.

[0082] Comparative Example

[0083] Inorganic glue is applied on the surface of 2mm thick veneer with a thickness of 0.2mm. The inorganic glue includes 50 parts of magnesium oxide, 5 parts of silicon dioxide powder, 10 parts of phosphoric acid aqueous solution, 35 parts of water, and 2 parts of magnesium chloride by mass. The dihydrogen phosphate is composed of potassium dihydrogen phosphate and sodium dihydrogen phosphate in a mass ratio of 1:2.

[0084] The six single boards were stacked and then cold pressed to obtain a composite board. During the cold pressing step, the pressure acting on the board was 32 kPa and the cold pressing time was 12 hours.

[0085] The composite board was dried at 90°C for 24 h.

[0086] The formaldehyde emission of the board obtained by the test is 0.006mg / m³. The sample was submerged in water and boiled for 10 minutes and then soaked for 6 hours. The static bending strength after soaking was 11.4MPa, and the size of the impact pit was 11.5mm. The fire resistance grade of the dried sample was B1 according to GB8624-2012.

[0087] The embodiment of the present application can produce a multi-layer solid wood board with strong adhesion, good boiling resistance, good moisture resistance, and the characteristic of non-sustainable combustion. No volatile organic matter is added in the production process, and formaldehyde is only released by the wood itself.

[0088] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0089] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A method for producing a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board, characterized in that: The steps include: Apply inorganic glue on the surface of the veneer; stacking a plurality of the single boards and then cold pressing them to obtain a composite board; Drying the composite board to obtain the nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board; By mass, the inorganic glue comprises 35-50 parts of magnesium oxide, 1-5 parts of silica aerogel, 1-2 parts of aluminum silicate fiber, 5-20 parts of dihydrogen phosphate, 5-10 parts of aluminum oxide, and 30-50 parts of water; The veneer is also pre-treated before being coated with the inorganic glue, and the pre-treatment steps include: Soak the veneer in a pretreatment solution; draining the veneer; The pretreatment solution comprises, by mass, 20 to 35 parts of aluminum dihydrogen phosphate, 10 to 20 parts of magnesium chloride, 0.5 to 1 part of boric acid, and 30 to 50 parts of water; The dihydrogen phosphate in the inorganic glue is aluminum dihydrogen phosphate, and the inorganic glue also contains 0.3 to 0.5 parts of boric acid; In the step of soaking the single board with the pretreatment liquid, the pressure is 100 kPa-150 kPa, the temperature is 100° C.-110° C., and the time is 10 h-20 h.

2. The method for producing a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board according to claim 1, characterized in that: In the step of drying the composite board, the drying temperature is 90° C.-160° C. and the drying time is 10 h-24 h.

3. The method for producing a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board according to claim 1, characterized in that: The magnesium oxide comprises 5% of light-burned magnesium oxide and 95% of dead-burned magnesium oxide by mass. The particle size distribution of the light-burned magnesium oxide is 15 μm-25 μm, and the particle size distribution of the dead-burned magnesium oxide is 150 μm-250 μm.

4. The method for producing a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board according to claim 3, characterized in that: The preparation steps of the inorganic glue include: Mixing the light-burned magnesium oxide and the silicon dioxide aerogel to obtain a mixed powder; Adding the boric acid and the aluminum dihydrogen phosphate into the water, and then sequentially adding the aluminum silicate fiber, the aluminum oxide and the dead-burned magnesium oxide under stirring at 150 rpm-200 rpm to obtain a mixed solution; The stirring speed is increased to 500 rpm-600 rpm, the mixed powder is added to the mixed solution, and stirring is continued for 5 min-10 min to obtain the inorganic glue.

5. The method for manufacturing a nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board according to claim 1, characterized in that: In the cold pressing step, the pressure acting on the plate is 16kPa-32kPa, and the cold pressing time is 6h-12h.

6. A nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board, characterized in that: The nano-cross-linked anti-seepage cold-pressed multi-layer solid wood board is made by the manufacturing method of any one of claims 1 to 5.