Preparation method of high-purity vanadium metal

By combining metallothermic reduction, ultra-high temperature smelting, and molten salt electrolysis, the problem of difficult slag-alloy separation was solved, enabling the preparation of high-purity metallic vanadium and meeting the high-purity requirements of aerospace and other fields.

CN117488105BActive Publication Date: 2026-11-24PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311764232.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-19
Publication Date
2026-11-24
Estimated Expiration
2043-12-19

AI Technical Summary

Technical Problem

In existing technologies, when using the metallothermic reduction method to smelt high-purity metallic vanadium, it is difficult to separate the slag from the alloy, resulting in low purity that cannot meet the high purity requirements of aerospace, nuclear energy industry and other fields.

Method used

A mixture of vanadium-containing raw materials, reducing agents, and additives is used to carry out a metal thermal reduction reaction, followed by smelting and refining in an ultra-high temperature smelting furnace, and finally further purification through molten salt electrolytic refining, using magnesium powder igniter and a specific molten salt system for treatment.

Benefits of technology

It effectively removes aluminum and other impurities, yielding high-purity metallic vanadium that meets the high-purity requirements of aerospace, nuclear energy industry and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117488105B_ABST
    Figure CN117488105B_ABST
Patent Text Reader

Abstract

This invention relates to the field of metal smelting technology, specifically to a method for preparing high-purity metallic vanadium. The method includes the following steps: mixing vanadium-containing raw materials, reducing agents, and additives in a ratio of 100:40–49:6–10 until homogeneous; then carrying out a metallothermic reduction reaction; after the reaction is complete and the product is cooled, removing the upper smelting slag to obtain preliminary metallic vanadium; placing the preliminary metallic vanadium in an ultra-high temperature smelting furnace for smelting and refining, first reducing the furnace pressure to 10–100 kJ / L. ‑4 At Pa, a protective gas is introduced to the target pressure, the heating power is turned on, and the power is slowly increased until the metal melts. After melting for 1 to 60 minutes, the metal is cooled to obtain metallic vanadium. The metallic vanadium is then refined by molten salt electrolysis to obtain high-purity metallic vanadium.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal smelting technology, and in particular to a method for preparing high-purity metallic vanadium. Background Technology

[0002] High-purity metallic vanadium refers to pure vanadium with a purity greater than 99.9%. It possesses characteristics such as high melting point, good processing performance, strong corrosion resistance, and a small fast neutron absorption cross section. It is mainly used in aerospace, nuclear energy, electronics, superconducting alloys, and special alloys. High-purity metallic vanadium has already achieved or has the potential for significant applications in important fields such as aerospace bearing steel, vanadium-based alloys for nuclear engineering, and vanadium-nickel alloy sputtering targets for integrated circuits. These fields have extremely high requirements for the purity of metallic vanadium.

[0003] Currently, the metallothermic reduction method for smelting metallic vanadium mainly uses a single reducing agent, resulting in slag with a high melting point, which is not conducive to the separation of slag and alloy. To address this technical problem, a method for preparing high-purity metallic vanadium is proposed. Summary of the Invention

[0004] To address the technical problems existing in the prior art, the present invention provides a method for preparing high-purity metallic vanadium.

[0005] To achieve the above objectives, the embodiments of the present invention provide the following technical solutions: In a first aspect, in one embodiment of the present invention, a method for preparing high-purity metallic vanadium is provided, the method comprising the following steps: The raw materials containing vanadium, reducing agent and additives are mixed evenly in a ratio of 100:40~49:6~10, and then a metallothermic reduction reaction is carried out. After the reaction is completed and the product is cooled, the upper smelting slag is removed to obtain preliminary metallic vanadium. The initial vanadium metal is placed in an ultra-high temperature smelting furnace for smelting and refining. The pressure inside the furnace is first reduced to 10-10. - 4 At Pa, a protective gas is introduced to the target pressure, the heating power is turned on, and the power is slowly increased until the metal melts. After melting for 1 to 60 minutes, the metal vanadium is obtained by cooling. High-purity vanadium is obtained by refining metallic vanadium through molten salt electrolysis.

[0006] As a further aspect of the present invention, the vanadium-containing raw material, reducing agent, and additives are mixed evenly in a ratio of 100:40-49:6-10, and then subjected to a metallothermic reduction reaction. After the reaction is completed and the product is cooled, the upper smelting slag is removed to obtain preliminary metallic vanadium, comprising: A metallic thermal reduction reaction occurs when magnesium powder is ignited as an igniter.

[0007] As a further embodiment of the present invention, the vanadium-containing raw material is vanadium pentoxide with a particle size of 0.5-6 mm.

[0008] As a further aspect of the present invention, the mass fractions of each chemical component in the vanadium-containing raw material are: V2O5≥99.9%, Fe≤0.02%, Si≤0.01%, Cr≤0.01%.

[0009] As a further aspect of the present invention, the mass fractions of each chemical component of the reducing agent are Al≥99.99%, Fe≤0.001%, Si≤0.001%, and Cr≤0.001%.

[0010] As a further embodiment of the present invention, the additive is alumina with a particle size of less than 0.1 to 3.

[0011] As a further embodiment of the present invention, the igniter is magnesium powder with a particle size of 160 mesh to 240 mesh.

[0012] As a further aspect of the present invention, the ultra-high temperature melting furnace includes a magnetic levitation induction furnace, an electron beam melting furnace, and an ion beam melting furnace.

[0013] As a further embodiment of the present invention, the molten salt system in molten salt electrolytic refining is NaCl-KCl-VCl2, NaCl-CaCl2-VCl2, or NaCl-LiCl-VCl2.

[0014] As a further aspect of the present invention, the molten salt electrolytic refining is carried out in a molten salt electrolytic refining structure.

[0015] The technical solution provided by this invention has the following beneficial effects: In this invention, vanadium-containing raw materials, reducing agents, and additives are mixed evenly and placed in a reaction vessel. A metallothermic reduction reaction is initiated by ignition with an igniter to obtain preliminary metallic vanadium. The preliminary metallic vanadium is then placed in a magnetic induction levitation furnace for smelting and refining to remove most of the aluminum and some of the remaining impurity elements, thus obtaining metallic vanadium. The metallic vanadium after magnetic induction levitation remelting and refining is further purified by molten salt electrolytic refining to obtain high-purity metallic vanadium.

[0016] These or other aspects of the invention will become more apparent from the following description of embodiments. It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only, and are not intended to limit the invention. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other embodiments can be obtained based on these drawings without creative effort.

[0018] Figure 1 This is a structural diagram of a molten salt electrolytic refining structure according to an embodiment of the present invention.

[0019] In the diagram: 1-Sealed outer shell, 2-Cathode, 3-Anode, 4-Insulating material, 5-Graphite tongs, 6-First graphite cover, 7-Second graphite cover. Detailed Implementation

[0020] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0021] The flowchart shown in the attached diagram is for illustrative purposes only and does not necessarily include all content and operations / steps, nor does it necessarily have to be performed in the order described. For example, some operations / steps can be broken down, combined, or partially merged, so the actual execution order may change depending on the actual situation.

[0022] This invention provides a method for preparing high-purity metallic vanadium, which includes the following steps: Step S1: Mix the vanadium-containing raw materials, reducing agent, and additives in a ratio of 100:40~49:6~10 evenly, and then carry out a metallothermic reduction reaction. After the reaction is completed and the product is cooled, remove the upper smelting slag to obtain preliminary metallic vanadium.

[0023] The metallothermic reduction reaction is carried out in a graphite crucible made of UHPC material. UHPC is an ultra-high strength cement-based material with high strength, high toughness, and low porosity.

[0024] In this embodiment of the invention, step S1 involves uniformly mixing vanadium-containing raw materials, reducing agents, and additives in a ratio of 100:40-49:6-10, followed by a metallothermic reduction reaction. After the reaction is completed and the product is cooled, the upper smelting slag is removed to obtain preliminary metallic vanadium, comprising: A metallic thermal reduction reaction occurs when magnesium powder is ignited as an igniter.

[0025] In this embodiment of the invention, the vanadium-containing raw material is vanadium pentoxide with a particle size of 0.5-6 mm.

[0026] In this embodiment of the invention, the mass fractions of each chemical component in the vanadium-containing raw material are: V2O5≥99.9%, Fe≤0.02%, Si≤0.01%, Cr≤0.01%.

[0027] In this embodiment of the invention, the reducing agent is metallic aluminum with a particle size of 0.5-6 mm, and the mass fractions of each chemical component of the reducing agent are Al≥99.99%, Fe≤0.001%, Si≤0.001%, and Cr≤0.001%.

[0028] In this embodiment of the invention, the additive is alumina with a particle size of less than 0.1 to 3, and the content of Al2O3 in the additive is ≥99.9%.

[0029] In this embodiment of the invention, the igniter is magnesium powder with a particle size of 160 mesh to 240 mesh.

[0030] Step S2: Place the preliminary metallic vanadium in an ultra-high temperature smelting furnace for smelting and refining. First, reduce the pressure inside the furnace to 10-10. -4 At Pa, a protective gas is introduced to the target pressure, the heating power is turned on, and the power is slowly increased until the metal melts. After melting for 1 to 60 minutes, the metal is cooled to obtain vanadium.

[0031] The target pressure can be set as needed.

[0032] In this embodiment of the invention, the ultra-high temperature melting furnace includes a magnetic levitation induction furnace, an electron beam melting furnace, and an ion beam melting furnace.

[0033] In this embodiment of the invention, smelting and refining are carried out in an ultra-high temperature smelting furnace at a temperature of 1900–2800°C.

[0034] In step S2, protective gas is introduced to the target pressure, which is 10. -2 ~10 4 Pa.

[0035] Step S3: Refine the metallic vanadium by molten salt electrolysis to obtain high-purity metallic vanadium.

[0036] In this embodiment of the invention, the molten salt system in the molten salt electrolytic refining is NaCl-KCl-VCl2, NaCl-CaCl2-VCl2, or NaCl-LiCl-VCl2. The most important salt in the molten salt system, VCl2, is prepared by reacting metallic vanadium with hydrogen chloride at 240℃ to 960℃. High-purity metallic vanadium is obtained after molten salt electrolytic refining.

[0037] The molten salt electrolytic refining is carried out in a molten salt electrolytic refining structure.

[0038] like Figure 1 As shown, specifically, the molten salt electrolytic refining structure includes a sealed outer shell 1 and a graphite tongs 5 ​​disposed inside the sealed outer shell 1. The graphite tongs 5 ​​has an opening at its upper part, and an insulating material 4 is disposed between the graphite tongs 5 ​​and the sealed outer shell 1. The graphite tongs 5 ​​is connected to the anode 3, and the cathode 2 is inserted into the graphite tongs 5 ​​through the upper opening. It also includes a first graphite cover 6 and a second graphite cover 7. The 6 covers the interface between the graphite tongs 5 ​​and the anode, and the second graphite cover 7 is suspended from the cathode 2 to cover the upper opening of the graphite tongs 5. This arrangement is mainly to prevent corrosion products from falling into the molten salt and causing contamination after the molten salt volatilizes and corrodes the sealed outer shell.

[0039] In this embodiment of the invention, the cathode 2 is a molybdenum rod, tungsten rod, iron rod, copper rod, or vanadium rod, and the anode 3 is metallic vanadium refined by magnetic induction suspension remelting.

[0040] This invention involves uniformly mixing vanadium-containing raw materials, reducing agents, and additives, placing them in a reaction vessel, and igniting them with an igniter to induce a metallothermic reduction reaction, thereby obtaining preliminary metallic vanadium. The preliminary metallic vanadium is then placed in a magnetic induction levitation furnace for smelting and refining to remove most of the aluminum and some of the remaining impurity elements, yielding metallic vanadium. The metallic vanadium after magnetic induction levitation remelting and refining is further purified by molten salt electrolysis to obtain high-purity metallic vanadium.

[0041] Example 1 A method for preparing high-purity metallic vanadium includes the following steps: Step S1: Mix the vanadium-containing raw materials, reducing agent, and additives in a ratio of 100:49:10 evenly, and then carry out a metallothermic reduction reaction. After the reaction is completed and the product is cooled, remove the upper smelting slag to obtain preliminary metallic vanadium.

[0042] The metallothermic reduction reaction is carried out in a graphite crucible made of UHPC material. UHPC is an ultra-high strength cement-based material with high strength, high toughness, and low porosity.

[0043] In this embodiment of the invention, step S1 involves uniformly mixing the vanadium-containing raw material, reducing agent, and additive in a ratio of 100:49:10, followed by a metallothermic reduction reaction. After the reaction is complete and the product is cooled, the upper smelting slag is removed to obtain preliminary metallic vanadium, comprising: A metallic thermal reduction reaction occurs when magnesium powder is ignited as an igniter.

[0044] In this embodiment of the invention, the vanadium-containing raw material is vanadium pentoxide with a particle size of 6 mm.

[0045] In this embodiment of the invention, the mass fractions of each chemical component in the vanadium-containing raw material are: V2O5≥99.9%, Fe≤0.02%, Si≤0.01%, Cr≤0.01%.

[0046] In this embodiment of the invention, the reducing agent is metallic aluminum with a particle size of 6 mm, and the mass fractions of each chemical component of the reducing agent are Al≥99.99%, Fe≤0.001%, Si≤0.001%, and Cr≤0.001%.

[0047] In this embodiment of the invention, the additive is aluminum oxide with a particle size smaller than that of anode 3, and the content of Al2O3 in the additive is ≥99.9%.

[0048] In this embodiment of the invention, the igniter is magnesium powder with a particle size of 240 mesh.

[0049] Step S2: Place the preliminary metallic vanadium in an ultra-high temperature smelting furnace for smelting and refining. First, pump the pressure inside the furnace to 10 Pa, then fill it with protective gas to the target pressure, turn on the heating power, and slowly increase the power until the metal melts. After smelting for 60 minutes, cool to obtain metallic vanadium.

[0050] In this embodiment of the invention, the ultra-high temperature melting furnace includes a magnetic levitation induction furnace, an electron beam melting furnace, and an ion beam melting furnace.

[0051] In this embodiment of the invention, smelting and refining are carried out in an ultra-high temperature smelting furnace at a smelting temperature of 2800°C.

[0052] In step S2, protective gas is introduced to the target pressure, which is 10. 4 Pa.

[0053] Step S3: Refine the metallic vanadium by molten salt electrolysis to obtain high-purity metallic vanadium.

[0054] In this embodiment of the invention, the molten salt system in the molten salt electrolytic refining is NaCl-KCl-VCl2, NaCl-CaCl2-VCl2, or NaCl-LiCl-VCl2.

[0055] Example 2 A method for preparing high-purity metallic vanadium includes the following steps: Step S1: Mix the vanadium-containing raw materials, reducing agent, and additives in a ratio of 100:40:6 evenly, and then carry out a metallothermic reduction reaction. After the reaction is completed and the product is cooled, remove the upper smelting slag to obtain preliminary metallic vanadium.

[0056] The metallothermic reduction reaction is carried out in a graphite crucible made of UHPC material. UHPC is an ultra-high strength cement-based material with high strength, high toughness, and low porosity.

[0057] In this embodiment of the invention, step S1 involves uniformly mixing the vanadium-containing raw material, reducing agent, and additive in a ratio of 100:40:6, then performing a metallothermic reduction reaction. After the reaction is completed and the product is cooled, the upper smelting slag is removed to obtain preliminary metallic vanadium, comprising: A metallic thermal reduction reaction occurs when magnesium powder is ignited as an igniter.

[0058] In this embodiment of the invention, the vanadium-containing raw material is vanadium pentoxide with a particle size of 0.5 mm.

[0059] In this embodiment of the invention, the mass fractions of each chemical component in the vanadium-containing raw material are: V2O5≥99.9%, Fe≤0.02%, Si≤0.01%, Cr≤0.01%.

[0060] In this embodiment of the invention, the reducing agent is metallic aluminum with a particle size of 0.5 mm, and the mass fractions of each chemical component of the reducing agent are Al≥99.99%, Fe≤0.001%, Si≤0.001%, and Cr≤0.001%.

[0061] In this embodiment of the invention, the additive is alumina with a particle size of less than 0.1 mm, and the content of Al2O3 in the additive is ≥99.9%.

[0062] In this embodiment of the invention, the igniter is magnesium powder with a particle size of 160 mesh.

[0063] Step S2: Place the preliminary metallic vanadium in an ultra-high temperature smelting furnace for smelting and refining. First, reduce the pressure inside the furnace to 10. -4 At Pa, a protective gas is introduced to the target pressure, the heating power is turned on, and the power is slowly increased until the metal melts. After melting the sealed shell for 1 minute, the metal vanadium is obtained by cooling.

[0064] In this embodiment of the invention, the ultra-high temperature melting furnace includes a magnetic levitation induction furnace, an electron beam melting furnace, and an ion beam melting furnace.

[0065] In this embodiment of the invention, smelting and refining are carried out in an ultra-high temperature smelting furnace at a smelting temperature of 1900°C.

[0066] In step S2, protective gas is introduced to the target pressure, which is 10. -2 Pa.

[0067] Step S3: Refine the metallic vanadium by molten salt electrolysis to obtain high-purity metallic vanadium.

[0068] In this embodiment of the invention, the molten salt system in the molten salt electrolytic refining is NaCl-KCl-VCl2, NaCl-CaCl2-VCl2, or NaCl-LiCl-VCl2.

[0069] Example 3 A method for preparing high-purity metallic vanadium includes the following steps: Step S1: Mix the vanadium-containing raw materials, reducing agent, and additives in a ratio of 100:47:9 evenly, and then carry out a metallothermic reduction reaction. After the reaction is completed and the product is cooled, remove the upper smelting slag to obtain preliminary metallic vanadium.

[0070] The metallothermic reduction reaction is carried out in a graphite crucible made of UHPC material. UHPC is an ultra-high strength cement-based material with high strength, high toughness, and low porosity.

[0071] In this embodiment of the invention, step S1 involves uniformly mixing the vanadium-containing raw material, reducing agent, and additive in a ratio of 100:47:9, followed by a metallothermic reduction reaction. After the reaction is complete and the product is cooled, the upper smelting slag is removed to obtain preliminary metallic vanadium, comprising: A metallic thermal reduction reaction occurs when magnesium powder is ignited as an igniter.

[0072] In this embodiment of the invention, the vanadium-containing raw material is vanadium pentoxide with a particle size of 4 mm, which is the size of insulating material.

[0073] In this embodiment of the invention, the mass fractions of each chemical component in the vanadium-containing raw material are: V2O5≥99.9%, Fe≤0.02%, Si≤0.01%, Cr≤0.01%.

[0074] In this embodiment of the invention, the reducing agent is metallic aluminum with a particle size of 4 mm (insulating material). The mass fractions of each chemical component of the reducing agent are Al ≥ 99.99%, Fe ≤ 0.001%, Si ≤ 0.001%, and Cr ≤ 0.001%.

[0075] In this embodiment of the invention, the additive is alumina with a particle size smaller than 2 mm of the cathode, and the content of Al2O3 in the additive is ≥99.9%.

[0076] In this embodiment of the invention, the igniter is magnesium powder with a particle size of 230 mesh.

[0077] Step S2: Place the preliminary metallic vanadium in an ultra-high temperature smelting furnace for smelting and refining. First, reduce the pressure inside the furnace to 10-10. -4 At Pa, a protective gas is introduced to the target pressure, the heating power is turned on, and the power is slowly increased until the metal melts. After melting for 1 to 60 minutes, the metal is cooled to obtain vanadium.

[0078] In this embodiment of the invention, the ultra-high temperature melting furnace includes a magnetic levitation induction furnace, an electron beam melting furnace, and an ion beam melting furnace.

[0079] In this embodiment of the invention, smelting and refining are carried out in an ultra-high temperature smelting furnace at a smelting temperature of 2600°C.

[0080] In step S2, protective gas is introduced to the target pressure, which is 10. -2 ~10 4 Pa.

[0081] Step S3: Refine the metallic vanadium by molten salt electrolysis to obtain high-purity metallic vanadium.

[0082] In this embodiment of the invention, the molten salt system in the molten salt electrolytic refining is NaCl-KCl-VCl2, NaCl-CaCl2-VCl2, or NaCl-LiCl-VCl2.

[0083] Example 4 A method for preparing high-purity metallic vanadium includes the following steps: Step S1: Mix the vanadium-containing raw materials, reducing agent, and additives in a ratio of 100:43:7 evenly, and then carry out a metallothermic reduction reaction. After the reaction is completed and the product is cooled, remove the upper smelting slag to obtain preliminary metallic vanadium.

[0084] The metallothermic reduction reaction is carried out in a graphite crucible made of UHPC material. UHPC is an ultra-high strength cement-based material with high strength, high toughness, and low porosity.

[0085] In this embodiment of the invention, step S1 involves uniformly mixing the vanadium-containing raw material, reducing agent, and additive in a ratio of 100:43:7, then performing a metallothermic reduction reaction. After the reaction is completed and the product is cooled, the upper smelting slag is removed to obtain preliminary metallic vanadium, comprising: A metallic thermal reduction reaction occurs when magnesium powder is ignited as an igniter.

[0086] In this embodiment of the invention, the vanadium-containing raw material is vanadium pentoxide with a particle size of 2 mm.

[0087] In this embodiment of the invention, the mass fractions of each chemical component in the vanadium-containing raw material are: V2O5≥99.9%, Fe≤0.02%, Si≤0.01%, Cr≤0.01%.

[0088] In this embodiment of the invention, the reducing agent is metallic aluminum with a particle size of 2 mm (cathode). The mass fractions of each chemical component of the reducing agent are Al ≥ 99.99%, Fe ≤ 0.001%, Si ≤ 0.001%, and Cr ≤ 0.001%.

[0089] In this embodiment of the invention, the additive is aluminum oxide with a particle size smaller than 1 mm of the sealed shell, and the content of Al2O3 in the additive is ≥99.9%.

[0090] In this embodiment of the invention, the igniter is magnesium powder with a particle size of 180 mesh to 230 mesh.

[0091] Step S2: Place the preliminary metallic vanadium in an ultra-high temperature smelting furnace for smelting and refining. First, reduce the pressure inside the furnace to 10-10. -4 At Pa, a protective gas is introduced to the target pressure, the heating power is turned on, and the power is slowly increased until the metal melts. After melting for 60 minutes, the metal is cooled to obtain vanadium.

[0092] In this embodiment of the invention, the ultra-high temperature melting furnace includes a magnetic levitation induction furnace, an electron beam melting furnace, and an ion beam melting furnace.

[0093] In this embodiment of the invention, smelting and refining are carried out in an ultra-high temperature smelting furnace at a smelting temperature of 2100°C.

[0094] In step S2, protective gas is introduced to the target pressure, which is 10. -2 Pa.

[0095] Step S3: Refine the metallic vanadium by molten salt electrolysis to obtain high-purity metallic vanadium.

[0096] In this embodiment of the invention, the molten salt system in the molten salt electrolytic refining is NaCl-KCl-VCl2, NaCl-CaCl2-VCl2, or NaCl-LiCl-VCl2.

[0097] Example 5 A method for preparing high-purity metallic vanadium includes the following steps: Step S1: Mix the vanadium-containing raw materials, reducing agent, and additives in a ratio of 100:45:8 evenly, and then carry out a metallothermic reduction reaction. After the reaction is completed and the product is cooled, remove the upper smelting slag to obtain preliminary metallic vanadium.

[0098] The metallothermic reduction reaction is carried out in a graphite crucible made of UHPC material. UHPC is an ultra-high strength cement-based material with high strength, high toughness, and low porosity.

[0099] In this embodiment of the invention, step S1 involves uniformly mixing the vanadium-containing raw material, reducing agent, and additive in a ratio of 100:45:8, then performing a metallothermic reduction reaction. After the reaction is completed and the product is cooled, the upper smelting slag is removed to obtain preliminary metallic vanadium, comprising: A metallic thermal reduction reaction occurs when magnesium powder is ignited as an igniter.

[0100] In this embodiment of the invention, the vanadium-containing raw material is vanadium pentoxide with a particle size of 3 (anode 3).

[0101] In this embodiment of the invention, the mass fractions of each chemical component in the vanadium-containing raw material are: V2O5≥99.9%, Fe≤0.02%, Si≤0.01%, Cr≤0.01%.

[0102] In this embodiment of the invention, the reducing agent is metallic aluminum with a particle size of 3 mm, and the mass fractions of each chemical component of the reducing agent are Al≥99.99%, Fe≤0.001%, Si≤0.001%, and Cr≤0.001%.

[0103] In this embodiment of the invention, the additive is alumina with a particle size of less than 1.5 mm, and the content of Al2O3 in the additive is ≥99.9%.

[0104] In this embodiment of the invention, the igniter is magnesium powder with a particle size of 200 mesh.

[0105] Step S2: Place the preliminary metallic vanadium in an ultra-high temperature smelting furnace for smelting and refining. First, reduce the pressure inside the furnace to 10-10. -4 At Pa, a protective gas is introduced to the target pressure, the heating power is turned on, and the power is slowly increased until the metal melts. After melting for 1 to 60 minutes, the metal is cooled to obtain vanadium.

[0106] In this embodiment of the invention, the ultra-high temperature melting furnace includes a magnetic levitation induction furnace, an electron beam melting furnace, and an ion beam melting furnace.

[0107] In this embodiment of the invention, smelting and refining are carried out in an ultra-high temperature smelting furnace at a smelting temperature of 2500°C.

[0108] In step S2, protective gas is introduced to the target pressure, which is 10. -2 ~10 4 Pa.

[0109] Step S3: Refine the metallic vanadium by molten salt electrolysis to obtain high-purity metallic vanadium.

[0110] In this embodiment of the invention, the molten salt system in the molten salt electrolytic refining is NaCl-KCl-VCl2, NaCl-CaCl2-VCl2, or NaCl-LiCl-VCl2.

[0111] Example 6 With the aim of preparing high-purity metallic vanadium, 10 kg of vanadium pentoxide (1-3 mm particle size), 4.45 kg of metallic aluminum (1-3 mm particle size), and 0.8 kg of alumina (180 mesh particle size) were mixed evenly and placed in a graphite crucible reaction vessel. A metallothermic reduction reaction was initiated by igniting with 200 mesh magnesium powder. After the reaction was completed and the product cooled, the upper smelting slag was removed to obtain preliminary metallic vanadium. The preliminary metallic vanadium was placed in an induction melting furnace with a vacuum of 6 × 10⁻² Pa and refined at 2600℃ for 30 min to obtain metallic vanadium. The vanadium refined by vacuum induction remelting was then refined by molten salt electrolysis using NaCl-CaCl₂-VCl₂. The cathode current density was controlled at 0.3 A / cm² during electrolysis to obtain high-purity metallic vanadium.

[0112] After the above operations, 4.2 kg of preliminary metallic vanadium was obtained, with the following composition: V: 93.62%, Al: 0.621%, O: 4.61%, N: 0.090%, C: 0.018%, Fe: 0.009%, Si: 0.010%, Cr: 0.010%; the composition of metallic vanadium was: V: 98.71%, Al: 0.007%, O: 1.11%, N: 0.058%, C: 0.018%, Fe: 0.007%, Si: 0.004%, Cr: 0.006%; and the composition of high-purity metallic vanadium was: V: 99.95%, Al: 0.004%, O: 0.022%, N: 0.003%, C: 0.008%, Fe: 0.004%, Si: 0.003%, Cr: 0.005%.

[0113] Example 7 With the aim of preparing high-purity metallic vanadium, 15 kg of vanadium pentoxide (1-3 mm particle size), 6.67 kg of metallic aluminum (1-3 mm particle size), and 1.2 kg of alumina (180 mesh particle size) were mixed evenly and placed in a graphite crucible reaction vessel. A metallothermic reduction reaction was initiated by ignition with 200 mesh magnesium powder. After the reaction was completed and the product cooled, the upper smelting slag was removed to obtain preliminary metallic vanadium. The preliminary metallic vanadium was placed in an induction melting furnace with a vacuum of 6 × 10⁻² Pa and refined at 2600℃ for 30 min to obtain metallic vanadium. The vanadium refined by vacuum induction remelting was then refined by molten salt electrolysis using NaCl-CaCl₂-VCl₂. The cathode current density was controlled at 0.35 A / cm² during electrolysis to obtain high-purity metallic vanadium.

[0114] After the above operations, 6.5 kg of preliminary metallic vanadium was obtained, with the following composition: V: 94.17%, Al: 0.912%, O: 3.80%, N: 0.081%, C: 0.014%, Fe: 0.009%, Si: 0.007%, Cr: 0.009%; the composition of metallic vanadium was: V: 98.92%, Al: 0.008%, O: 0.92%, N: 0.042%, C: 0.016%, Fe: 0.006%, Si: 0.003%, Cr: 0.006%; and the composition of high-purity metallic vanadium was: V: 99.96%, Al: 0.004%, O: 0.012%, N: 0.004%, C: 0.009%, Fe: 0.003%, Si: 0.004%, Cr: 0.004%.

[0115] Example 8 With the aim of preparing high-purity metallic vanadium, 15 kg of vanadium pentoxide (1-3 mm particle size), 6.67 kg of metallic aluminum (1-3 mm particle size), and 1.2 kg of alumina (180 mesh particle size) were mixed evenly and placed in a graphite crucible reaction vessel. A metallothermic reduction reaction was initiated by igniting with 200 mesh magnesium powder. After the reaction was completed and the product cooled, the upper smelting slag was removed to obtain preliminary metallic vanadium. The preliminary metallic vanadium was placed in an induction melting furnace with a vacuum degree of 3 × 10⁻² Pa and refined at 2700℃ for 30 min to obtain metallic vanadium. The vanadium refined by vacuum induction remelting was then refined by molten salt electrolysis using NaCl-LiCl-VCl₂. The cathode current density was controlled at 0.4 A / cm² during electrolysis to obtain high-purity metallic vanadium.

[0116] After the above operations, 6.3 kg of preliminary metallic vanadium was obtained, with the following composition: V: 94.53%, Al: 0.423%, O: 4.11%, N: 0.091%, C: 0.016%, Fe: 0.008%, Si: 0.008%, Cr: 0.007%; the composition of metallic vanadium was: V: 98.64%, Al: 0.007%, O: 1.12%, N: 0.044%, C: 0.012%, Fe: 0.005%, Si: 0.003%, Cr: 0.005%; and the composition of high-purity metallic vanadium was: V: 99.96%, Al: 0.003%, O: 0.015%, N: 0.003%, C: 0.007%, Fe: 0.003%, Si: 0.003%, Cr: 0.004%.

[0117] The present invention also provides vanadium composition tables for each stage of Examples 6, 7 and 8, as follows: Vanadium metal composition (%) in each stage of Examples 6, 7, and 8

[0118] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention.

Claims

1. A method for preparing high-purity metallic vanadium, characterized in that, The preparation method includes: The raw materials containing vanadium, reducing agent, and additives are mixed evenly in a ratio of 100:40~49:6~10, and then a metallothermic reduction reaction is carried out. After the reaction is completed and the product is cooled, the upper smelting slag is removed to obtain preliminary metallic vanadium. The metallothermic reduction reaction is then carried out by ignition with magnesium powder as an igniter. The initial vanadium metal is placed in an ultra-high temperature smelting furnace for smelting and refining. The pressure inside the furnace is first reduced to 10-10. -4 At a pressure of 10 Pa, a protective gas is introduced to the target pressure, the heating power is turned on, and the power is slowly increased until the metal melts. After melting for 1–60 minutes, the metal is cooled to obtain metallic vanadium. The target pressure is 10 Pa. -2 ~10 4 Pa, melting temperature is 1900~2800℃; High-purity vanadium metal is obtained by molten salt electrolytic refining of metallic vanadium. The molten salt system in the molten salt electrolytic refining is NaCl-KCl-VCl2, NaCl-CaCl2-VCl2, or NaCl-LiCl-VCl2. The salt VCl2 in the molten salt system is prepared by reacting metallic vanadium with hydrogen chloride at 240℃ to 960℃. The molten salt electrolytic refining is carried out in a molten salt electrolytic refining structure, which includes a sealed outer shell and a graphite tong pot disposed inside the sealed outer shell. The graphite tong pot has an opening at its upper part, and an insulating material is disposed between the graphite tong pot and the sealed outer shell. The graphite tong pot is connected to the anode, and the cathode is inserted into the graphite tong pot through the opening at the upper part of the graphite tong pot. It also includes a first graphite cover and a second graphite cover. The first graphite cover covers the interface between the graphite tong pot and the anode, and the second graphite cover is suspended from the cathode to cover the opening at the upper part of the graphite tong pot.

2. The method for preparing high-purity metallic vanadium as described in claim 1, characterized in that, The vanadium-containing raw material is vanadium pentoxide with a particle size of 0.5–6 mm.

3. The method for preparing high-purity metallic vanadium as described in claim 1, characterized in that, The mass fractions of each chemical component in the vanadium-containing raw material are: V2O5≥99.9%, Fe≤0.02%, Si≤0.01%, Cr≤0.01%.

4. The method for preparing high-purity metallic vanadium as described in claim 1, characterized in that, The reducing agent has the following chemical components by mass: Al ≥ 99.99%, Fe ≤ 0.001%, Si ≤ 0.001%, and Cr ≤ 0.001%.

5. The method for preparing high-purity metallic vanadium as described in claim 1, characterized in that, The additive is aluminum oxide.

6. The method for preparing high-purity metallic vanadium as described in claim 2, characterized in that, The igniter is magnesium powder with a particle size of 160-240 mesh.

7. The method for preparing high-purity metallic vanadium as described in claim 1, characterized in that, The ultra-high temperature melting furnace includes a magnetic levitation induction furnace, an electron beam melting furnace, and an ion beam melting furnace.

Citation Information

Patent Citations

  • Preparation method of low-impurity vanadium-aluminum alloy

    CN105886869A

  • Method for preparing high-purity metal vanadium

    CN116005011A

  • High-purity vanadium obtaining method