A method of improving the low temperature impact toughness of a heat treated rail
By optimizing the chemical composition and heat treatment process of the rails and adopting a combination of air mist and wind cooling, the problem of insufficient low-temperature impact toughness of existing heat-treated rails has been solved, thus improving their service performance in cold regions.
Patent Information
- Application Number
- CN202311603166.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-28
AI Technical Summary
Existing heat-treated steel rails lack sufficient impact toughness in low-temperature environments, and cannot meet higher performance requirements, especially when used in high-altitude and cold regions.
By optimizing the chemical composition and heat treatment process of the rails, controlling the chemical composition content of the rails, and using a mixture of air mist and wind cooling during the heat treatment process, the grains are refined, the ductile-brittle transition temperature is reduced, and the low-temperature impact toughness is improved.
It significantly improves the impact energy of the rail at -40℃, reaching over 30J, meeting the service requirements of cold regions. It also has high tensile strength and elongation, and the Brinell hardness reaches over 330HB.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgical materials, and specifically relates to a method for improving the low-temperature impact toughness of heat-treated steel rails. Background Technology
[0002] Although there are relevant literatures on the low-temperature impact performance of steel rails both domestically and internationally, such as patent document CN109402520A (hereinafter referred to as document 1), which discloses a rare earth-containing low-temperature wear-resistant heat-treated steel rail and its preparation method, the heat-treated steel rail produced by this method has good tensile strength, tread hardness, and high impact energy at low temperatures. However, its impact energy at -40℃ (A) KU2 The notch size is only 15-20J. With the increase in railway transportation volume, rails used in low-temperature environments have new requirements for low-temperature toughness.
[0003] These objective conditions necessitate superior low-temperature performance of rails, particularly for enhanced operational capabilities in frigid regions. This significantly increases the performance requirements for rails operating in low-temperature environments, including higher demands on their low-temperature impact toughness. Therefore, developing rails with superior low-temperature impact toughness is of paramount importance for both production and economics. Summary of the Invention
[0004] To address one or more of the problems existing in the prior art, in one aspect of the present invention, a method for improving the low-temperature impact toughness of heat-treated steel rails is provided, comprising: controlling the chemical composition content of the steel rail, by mass percentage, to be: C 0.55-0.69%; Si 0.25-0.65%; Mn 0.65-1.10%; P ≤ 0.025%; S ≤ 0.025%; Cr 0.10-0.50%; RE 0.002-0.02%; with the remainder being Fe and unavoidable impurities; wherein the added Cr element can improve the hardenability and toughness of the steel, and the added RE element is a rare earth alloy, forming rare earth sulfur oxides and reducing the formation of other metallic sulfur compounds, resulting in minimal or no deformation during rolling, thus refining the grains in the steel. Simultaneously, the appropriate amount of rare earth in the steel material can lower the ductile-brittle transition temperature, which is of significant technical importance for the service of the steel rail in low-temperature regions; and
[0005] During the heat treatment process of the rail: after the final rolling, the residual heat treatment temperature is controlled at 830℃~850℃, and the rail exits the heat treatment production line after 110~130s of online heat treatment; in the first stage online, the top surface, both sides, lower jaw of the gauge angle, and bottom of the rail head are cooled by air mist, with an actual cooling rate of 3~5℃ / s and a cooling time of 50~80s; in the second stage, weak cooling is performed on the top surface, both sides of the rail head, lower jaw of the gauge angle, and bottom of the rail by air mist, with a cooling rate ≤2℃ / s. After cooling, the exit rail head temperature is 450℃~500℃, and then it is naturally air-cooled to room temperature.
[0006] In some embodiments, the -40°C impact energy A of the heat-treated rail is... KU2 It is above 30J.
[0007] In some embodiments, the chemical composition of the rail is controlled in the steelmaking process to be as follows by mass percentage: C 0.62-0.65%; Si 0.45-0.53%; Mn 0.92-1.05%; P≤0.020%; S≤0.010%; Cr 0.12-0.16%; RE 0.002-0.01%; with the remainder being Fe and unavoidable impurities.
[0008] In some embodiments, the steelmaking process includes: molten iron → converter smelting → LF refining → VD → continuous casting; wherein: the converter smelting adopts aluminum-free deoxidation alloying, and the whole process is carried out by normal argon blowing as in refining; the vacuum degree is ≤0.10KPa, the deep vacuum time is ≥15min, the superheat ΔT is ≤30℃, and the rare earth alloy is added at the VD station.
[0009] In some embodiments, the method further includes a rail rolling process, which includes: billet → sawing → heating → BD1 rolling → BD2 rolling → continuous rolling on a CCS universal mill; wherein: the temperature of the billet heating and preheating section is not greater than 830°C; the heating time is not less than 3 hours and 15 minutes; the furnace exit temperature is not less than 1150°C, the initial rolling temperature is ≥1100°C, and the final rolling temperature is 910~940°C.
[0010] In some embodiments, during the heat treatment of the rail, the online residual heat quenching cooling medium is a mixture of gas mist and air.
[0011] On the other hand, the present invention provides a heat-treated steel rail, which is produced by the above-described method.
[0012] In some embodiments, the -40°C impact energy A of the heat-treated rail is... KU2 It is above 30J.
[0013] In some embodiments, the heat-treated rail has a tensile strength of 1032 MPa or higher, an elongation δ of 15% or higher, and an average Brinell hardness of 330 HB or higher.
[0014] Based on the above technical solutions, this invention, by optimizing the chemical composition of the rail and combining it with an optimized heat treatment process, can further improve the low-temperature impact toughness of the rail, thereby increasing the rail's impact energy (A) at -40℃. KU2 The J value reaches over 30J, significantly higher than the low-temperature impact toughness of the heat-treated rails produced in Reference 1. Therefore, the rails produced by the method of this invention can be used in high-altitude and cold environments. Detailed Implementation
[0015] In the following description, only certain exemplary embodiments are briefly described. As those skilled in the art will recognize, the described embodiments can be modified in various ways without departing from the spirit or scope of the invention. Therefore, the description is considered to be exemplary in nature and not restrictive.
[0016] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.
[0017] Example:
[0018] The steelmaking process is as follows: molten iron → converter smelting → LF refining → VD → continuous casting. Converter smelting employs aluminum-free deoxidation alloying, with argon blowing throughout the refining process; vacuum degree ≤ 0.10 kPa, deep vacuum time ≥ 15 min, superheat ΔT ≤ 30℃, and rare earth alloys are added at the VD station. The chemical compositions of each embodiment are shown in Table 1 below.
[0019] Table 1: Components and mass percentages (%) of each embodiment
[0020]
[0021] The rail rolling process is as follows: billet → sawing → heating → BD1 rolling → BD2 rolling → continuous rolling on the CCS universal mill. The temperature of the billet preheating section shall not exceed 830℃; the heating time shall not be less than 3 hours and 15 minutes. The furnace exit temperature shall not be lower than 1150℃, the initial rolling temperature shall be ≥1100℃, and the final rolling temperature shall be 910~940℃.
[0022] The heat treatment process is as follows: the online residual heat quenching cooling medium is a mixture of air mist and air. After the final rolling of the rail, the residual heat treatment temperature is controlled at 830℃~850℃, and the rail exits the heat treatment production line after 110~130s of online heat treatment. In the first stage online, air mist cooling is used on the top surface, sides, lower jaw of the gauge angle, and bottom of the rail head. The actual cooling rate of the cooling section is 3~5℃ / s, and the cooling time is 50~80s. In the second stage, weak cooling is used on the top surface, sides, lower jaw of the gauge angle, and bottom of the rail head. The cooling rate is ≤2℃ / s. After cooling, the exit rail head temperature is 450℃~500℃, and then it is naturally air-cooled to room temperature.
[0023] The heat treatment process parameters for Examples 1-3 are shown in Table 2 below. Comparative Example 1 was designed to heat treat the rails rolled in Example 1. The only difference is that the residual heat treatment temperature after the final rolling of the rails is 770℃, and the rails exit the heat treatment production line after 140s of online heat treatment. In the first stage of online heat treatment, the top surface, both sides, lower jaw of the gauge angle, and the bottom of the rails are cooled by air mist. The actual cooling rate of the cooling section is 4℃ / s, and the cooling time is 50-80s. In the second stage, weak cooling is used to cool the top surface, both sides of the rails, lower jaw of the gauge angle, and the bottom of the rails by air mist. The cooling rate is ≤2℃ / s. The exit rails temperature after cooling is 550℃, and then the rails are naturally air-cooled to room temperature.
[0024] Table 2: Heat treatment process parameters of Examples 1-3 and Comparative Example 1
[0025]
[0026] Performance of rolled steel samples: Tensile test specimens were prepared with a diameter d0 = 10 mm and a gauge length Lo = 5 do. Tread surface hardness was measured by random sampling on the rail, with a specimen length of 250 mm. 0.5 mm of the rail head was ground off the top surface. Five test points were used for Brinell hardness testing, and the average value was calculated. The test temperature was 20℃ ± 5℃. The sampling method, location, and dimensions of the above samples conformed to TB / T2344-2012 standard. Impact sampling was performed according to GB / T229-2007. The sampling location was at the center of the tread surface, in the longitudinal direction, with dimensions of 10 mm × 10 mm × 50 mm, classified as A. KU2 Type notch. The experimental results are shown in Table 3.
[0027] Table 3: Mechanical property test results of rails in various embodiments and comparative examples
[0028]
[0029] As can be seen from Table 3 above, the rails in all embodiments exhibit good low-temperature impact toughness, with A measured at -40℃. KU2The impact energy of the notched specimen can reach more than 30J, and it also has high tensile strength (more than 1030MPa), elongation δ (more than 15%) and average Brinell hardness (more than 330HB, preferably more than 331HB). Although Comparative Example 1 also adopted the composition design of Example 1, its heat treatment process is different from that of the present invention, and the low-temperature impact toughness of the rail produced by it is significantly lower than that of the present invention.
[0030] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for improving the low-temperature impact toughness of heat-treated steel rails, characterized in that, The method includes: (1) Steelmaking production process In the steelmaking process, the chemical composition of the rails is controlled as follows (by mass percentage): C 0.62–0.65%; Si 0.45–0.53%; Mn 0.92–1.05%; P ≤ 0.020%; S ≤ 0.010%; Cr 0.12–0.16%; RE 0.002–0.01%; the remainder being Fe and unavoidable impurities. The steelmaking process includes: molten iron → converter smelting → LF refining → VD → continuous casting. The converter smelting employs aluminum-free deoxidation alloying, and the entire process is carried out using normal argon blowing during refining. The vacuum degree is ≤ 0.10 kPa, the deep vacuum time is ≥ 15 min, the superheat ΔT is ≤ 30 °C, and rare earth alloys are added at the VD station. (2) Rail rolling process The rail rolling process includes: billet → sawing → heating → BD1 rolling → BD2 rolling → continuous rolling on a CCS universal mill; wherein: the billet preheating temperature is not higher than 830℃; the heating time is not less than 3 hours and 15 minutes; the furnace exit temperature is not lower than 1150℃, the initial rolling temperature is ≥1100℃, and the final rolling temperature is 910~940℃; and (3) Heat treatment process In the heat treatment process of the rail, the residual heat treatment temperature after the final rolling is controlled at 830℃~850℃, and the rail exits the heat treatment production line after 110~130 s of online heat treatment. In the first stage of online heat treatment, the top surface, both sides, lower jaw of the gauge angle, and bottom of the rail head are cooled by air mist, with an actual cooling rate of 3~5℃ / s and a cooling time of 50~80s. In the second stage of weak cooling, the top surface, both sides of the rail head, lower jaw of the gauge angle, and bottom of the rail are cooled by air mist, with a cooling rate of ≤2℃ / s. After cooling, the exit rail head temperature is 450℃~500℃, and then it is naturally air-cooled to room temperature. The -40℃ impact energy A of the heat-treated steel rail KU2 It has a tensile strength of 30 J or higher, a tensile strength of 1032 MPa or higher, an elongation δ of 15% or higher, and an average Brinell hardness of 330 HB or higher.
2. A heat-treated steel rail, which is produced by the method of claim 1.
Citation Information
Patent Citations
Rare earth-containing low temperature-resistant wear-resistant heat-treated rail and preparation method thereof
CN109402520A
Production method of low-temperature-resistant steel rail in alpine region
CN114635072A
Heat treatment method for improving low-temperature toughness of pearlite steel rail
CN115466833A