A simple preparation method of modified waste tire rubber, the product and application thereof in cement mortar

By modifying waste tire rubber with tannic acid and nano-titanium dioxide, the problem of poor compatibility between rubber and cement-based materials has been solved, a simple and efficient modification process has been achieved, the mechanical and photocatalytic properties of rubber-cement composite materials have been improved, and their application range has been expanded.

CN117511021BActive Publication Date: 2026-11-24WUHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311292638.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-07
Publication Date
2026-11-24
Estimated Expiration
2043-10-07

AI Technical Summary

Technical Problem

Existing chemical modification processes are cumbersome and energy-intensive, resulting in poor compatibility between waste rubber and cement-based materials, which limits their application in civil engineering.

Method used

A method for modifying waste tire rubber using tannic acid and nano-titanium dioxide was developed. By stirring and mixing at room temperature, the self-polymerization reaction of tannic acid and the photocatalytic properties of nano-titanium dioxide were utilized to improve the hydrophilicity of the rubber and its chemical bonding with cement.

Benefits of technology

The modification process has been simplified, the mechanical properties and photocatalytic properties of rubber-composite cementitious materials have been improved, and their application range in air purification, water purification, self-purification, sterilization and deodorization has been expanded.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117511021B_ABST
    Figure CN117511021B_ABST
Patent Text Reader

Abstract

The application discloses a simple preparation method of modified waste tire rubber, a finished product and application of the finished product in cement mortar, and belongs to the technical field of rubber derivative compositions. The application comprises the following steps: (1) adding waste tire rubber into a tannic acid aqueous solution and mixing, adjusting the pH of the obtained mixed solution through an alkaline solution to obtain a pre-reaction solution; (2) adding titanium dioxide into the pre-reaction solution and performing reaction, and obtaining a reaction mixture after the reaction is completed; (3) filtering the reaction mixture to obtain a filter cake, and washing and drying the filter cake to obtain modified waste tire rubber. The process is simple, the processing condition is mild, the hydrophilicity of the rubber can be obviously improved, and the mechanical properties and photocatalytic properties of the modified rubber composite cement-based material are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of rubber derivative composition technology, and more particularly to a simple method for preparing modified waste tire rubber, the finished product, and its application in cement mortar. Background Technology

[0002] The rapid development of the rubber industry has generated a large amount of waste rubber. In recent years, green building materials—rubber-cement based materials—have emerged, providing a new way to recycle waste rubber. Rubber-cement based materials can not only turn pulverized waste rubber particles into valuable resources, but also improve the toughness, freeze-thaw resistance, impact resistance, sound insulation, and thermal insulation performance of cement-based materials, meeting the needs of energy conservation, emission reduction, and promoting green environmental protection. However, rubber-cement based materials have a major drawback: the hydrophobic rubber has poor compatibility with the hydrophilic cement-based materials. To solve the compatibility problem between rubber and cement materials and thus improve the beneficial properties of rubber-cement based materials, chemical modification of rubber is necessary. However, due to the cumbersome and energy-intensive nature of some chemical modification processes, the application of rubber in the field of civil engineering has been greatly limited. Summary of the Invention

[0003] In view of the above-mentioned deficiencies of the prior art, in a first aspect of the present invention, a method for preparing modified waste tire rubber with simple process and mild processing conditions is provided, comprising the following steps: (1) Add waste tire rubber to tannic acid aqueous solution and mix. Adjust the pH of the resulting mixture with alkaline solution to obtain a pre-reaction solution; (2) Add titanium dioxide to the pre-reaction solution and react. After the reaction is completed, a reaction mixture is obtained. (3) The reaction mixture is filtered to obtain a filter cake, which is then washed and dried to obtain modified waste tire rubber.

[0004] In this invention, waste tire rubber is widely available. To improve reaction efficiency, its specific surface area can be altered, and suitable waste tire rubber forms, such as rubber blocks, rubber granules, or rubber powder, can be selected according to actual processing needs. Tannic acid, extracted from plants, is inexpensive and highly effective in modification. As a natural binder, tannic acid adheres titanium dioxide to the rubber surface while improving its hydrophilicity. Titanium dioxide possesses highly efficient photocatalytic properties, endowing the modified rubber with excellent photocatalytic capabilities. Photocatalysis can oxidize and decompose various organic compounds and some inorganic substances, destroying bacterial cell membranes and viral proteins to kill bacteria, and decomposing organic pollutants into harmless water and carbon dioxide. This facilitates the application of modified waste tire rubber in air purification, water purification, self-purification, sterilization and deodorization, anti-fog and anti-fogging fields, expanding its application scope.

[0005] In the modification process, the modification effect of the finished product can be optimized by controlling the proportion of raw materials. Preferably, the mass ratio of waste tire rubber, tannic acid, and titanium dioxide is 20:1:1~2. The concentration of tannic acid aqueous solution will affect the rubber treatment. If the concentration is too low or too high, the performance of the finished product will be reduced. Therefore, it should be controlled within a suitable range. Preferably, in step (1), the concentration of tannic acid aqueous solution is 5~10 g / L. Tannic acid molecules can undergo self-polymerization reaction at a suitable pH. This reaction can improve the hydrophilicity of the rubber surface and enhance the chemical bond between the modified rubber and cement. Preferably, in step (1), the pH of the mixture is adjusted to 8.0±0.2. Under the premise of achieving the purpose of adjusting pH to promote self-polymerization, the type and concentration of alkaline solution can be selected in various ways. Among them, aqueous solutions of sodium hydroxide and potassium hydroxide are particularly suitable. Preferably, in step (1), the alkaline solution is an aqueous solution of sodium hydroxide or potassium hydroxide, and the concentration of the alkaline solution is 0.1~0.5 mol / L.

[0006] Reducing the particle size of titanium dioxide helps to disperse it and improve its photocatalytic reaction performance. Nano-sized titanium dioxide can better meet the design requirements of this invention. Preferably, in step (2), the particle size of the titanium dioxide is <100nm. When tannic acid undergoes self-polymerization, it is used simultaneously with nano-titanium dioxide. At this time, tannic acid also acts as a binder to adhere the nano-titanium dioxide to the rubber surface. Nano-titanium dioxide has high-efficiency photocatalytic performance, and tannic acid has the function of improving hydrophilicity and chemical activity. Therefore, modifying rubber with tannic acid and nano-titanium dioxide can enhance the chemical bonding of rubber particles in cement and endow cement materials with photocatalytic performance. More importantly, this reaction process does not require energy consumption and only requires simple stirring and mixing at room temperature. Preferably, in step (2), the reaction is carried out at room temperature for 12~16h.

[0007] In a second aspect of the invention, a modified waste tire rubber is provided, prepared using the method of the first aspect of the invention.

[0008] In a third aspect of the invention, an application of the modified waste tire rubber of the second aspect of the invention is provided, specifically its application as a fine aggregate in the preparation of concrete.

[0009] Compared with the prior art, the present invention has the following advantages and beneficial effects: This invention provides a method for preparing modified waste tire rubber. The process is simple and the processing conditions are mild. It can significantly improve the hydrophilicity of rubber and effectively improve the mechanical properties and photocatalytic properties of modified rubber composite cementitious materials.

[0010] This invention provides a modified waste tire rubber that has good hydrophilicity and photocatalytic properties, and good compatibility with cement-based materials.

[0011] The present invention also provides the application of modified waste tire rubber as a fine aggregate in the preparation of concrete, which can improve the mechanical strength of concrete. Attached Figure Description

[0012] Figure 1 This is a schematic diagram of the application process in Example 4; Figure 2 A bar chart comparing the 28-day flexural strength of rubber-composite cement mortar and modified rubber-composite cement mortar; Figure 3 A bar chart comparing the 28-day compressive strength of rubber-composite cement mortar and modified rubber-composite cement mortar; Figure 4 A comparison of the photocatalytic degradation curves of methylene blue in rubber-composite cement mortar and modified rubber-composite cement mortar. Detailed Implementation

[0013] The present invention is further illustrated below by way of embodiments, but the invention is not limited to the scope of the embodiments described herein. Experimental methods in the following embodiments that do not specify specific conditions were performed according to conventional methods and conditions, or as selected according to the product instructions.

[0014] In the following embodiments: Nano-sized titanium dioxide, with a particle size of <100nm; Natural river sand, fineness: 2.3.

[0015] Example 1 A method for preparing modified waste tire rubber: (1) Weigh waste tire rubber powder, tannic acid and nano titanium dioxide in a weight ratio of 20:1:1; prepare a NaOH aqueous solution with a concentration of 0.1 mol / L; dissolve tannic acid in distilled water to prepare a tannic acid aqueous solution with a concentration of 10 g / L; add waste tire rubber powder to the tannic acid aqueous solution and stir to mix to obtain a mixture; adjust the pH of the mixture to 8 with NaOH aqueous solution to obtain a pre-reaction solution; (2) Add nano-titanium dioxide to the pre-reaction solution and stir the reaction at room temperature for 12 hours. After the reaction is completed, a reaction mixture is obtained. (3) The reaction mixture is filtered with a microporous membrane, the filter cake is collected, the filter cake is washed with distilled water, and finally dried in a forced-air drying oven at 60°C to obtain modified waste tire rubber.

[0016] Example 2 A method for preparing modified waste tire rubber: (1) Weigh waste tire rubber powder, tannic acid and nano titanium dioxide in a weight ratio of 20:1:2; prepare a NaOH aqueous solution with a concentration of 0.5 mol / L; dissolve tannic acid in distilled water to prepare a tannic acid aqueous solution with a concentration of 5 g / L; add waste tire rubber powder to the tannic acid aqueous solution and stir to mix to obtain a mixture; adjust the pH of the mixture to 7.8 with NaOH aqueous solution to obtain a pre-reaction solution; (2) Add nano-titanium dioxide to the pre-reaction solution and stir the reaction at room temperature for 16 hours. After the reaction is completed, a reaction mixture is obtained. (3) The reaction mixture is filtered with a microporous membrane, the filter cake is collected, the filter cake is washed with distilled water, and finally dried in a forced-air drying oven at 60°C to obtain modified waste tire rubber.

[0017] Example 3 (1) Weigh waste tire rubber powder, tannic acid and nano titanium dioxide in a weight ratio of 20:1:1.5 respectively; prepare a NaOH aqueous solution with a concentration of 0.3mol / L; dissolve tannic acid in distilled water to prepare a tannic acid aqueous solution with a concentration of 7.5g / L; add waste tire rubber powder to the tannic acid aqueous solution and stir to mix to obtain a mixture; adjust the pH of the mixture to 8.2 with NaOH aqueous solution to obtain a pre-reaction solution; (2) Add nano-titanium dioxide to the pre-reaction solution and stir the reaction at room temperature for 14 hours. After the reaction is completed, a reaction mixture is obtained. (3) The reaction mixture is filtered with a microporous membrane, the filter cake is collected, the filter cake is washed with distilled water, and finally dried in a forced-air drying oven at 60°C to obtain modified waste tire rubber.

[0018] Example 4 The modified waste tire rubber prepared in Example 1 was used as the experimental group, and the unmodified waste tire rubber powder was used as the control group. Both were applied to the preparation of concrete cement mortar. The cement used in the mortar was PO42.5 Portland cement, with a water-cement ratio of 0.5 and a cement-sand ratio of 2.5. Natural river sand was used as the fine aggregate. The experimental group and the control group replaced the fine aggregate with different volume percentages (5%, 10%, and 15%), respectively, to obtain the corresponding rubber-cement composite cement mortar and modified rubber-cement composite cement mortar.

[0019] After the rubber-cement composite cement mortar was poured and cured using methods commonly used in the field, its flexural strength and compressive strength were measured after 28 days.

[0020] The test results of 28-day flexural strength are as follows Figure 2 As shown. By Figure 2It can be seen that the 28-day flexural strengths of rubber composite cement mortar with 5%–15% unmodified rubber are 5.06 MPa, 4.48 MPa, and 3.42 MPa, respectively. The 28-day flexural strengths of modified rubber composite cement mortar with 5%–15% waste tire rubber are 5.97 MPa, 4.91 MPa, and 4.11 MPa, respectively. From the flexural strength data, it can be seen that the flexural strength of rubber composite cement mortar with modified rubber is increased by 15%–20% compared to rubber composite cement mortar with the same amount of unmodified rubber.

[0021] The test results of 28-day compressive strength are as follows Figure 3 As shown. By Figure 2 It can be seen that the 28-day compressive strengths of rubber composite cement mortar with 5%~15% unmodified rubber are 31.0 MPa, 22.2 MPa, and 16.1 MPa, respectively. The 28-day compressive strengths of rubber composite cement mortar with 5%~15% modified rubber are 35.5 MPa, 30.7 MPa, and 18.5 MPa, respectively. From the compressive strength data, it can be seen that the compressive strength of rubber composite cement mortar with modified rubber is increased by 15%~25% compared to rubber composite cement mortar with the same amount of unmodified rubber.

[0022] The results of these two tests show that the mechanical properties of the modified waste rubber composite cement mortar have been significantly improved.

[0023] Example 5 The photodegradation performance of methyl blue under ultraviolet light was tested in rubber-cement composite cement mortar and modified rubber-cement composite cement mortar prepared by adding 10% (by volume) of fine aggregate as a substitute in Example 4. To evaluate the photodegradation efficiency of the modified rubber-cement composite cement sample, a square sample measuring 40mm × 40mm × 40mm was immersed in 100mL of a methyl bromide solution with a contaminant concentration of 20mg / L. Before immersion, the cement sample was dried in the dark at room temperature for 24 hours. The photocatalytic degradation process was carried out under simulated natural ultraviolet irradiation using an irradiance of 10W / m². 2 The ultraviolet lamp was activated. 2 mL samples were collected from the methyl bromide solution at different time intervals until the end of the experiment. Finally, the photodegradation efficiency of the cement samples to the methyl bromide solution was determined using a UV-Vis spectrophotometer. The photodegradation curve of methylene blue under ultraviolet light is shown below. Figure 4 As shown.

[0024] Depend on Figure 4 It can be seen that the efficiency of removing methylene blue in rubber composite cement mortar with unmodified rubber after 12 hours of ultraviolet light irradiation is only 43.6%. However, the efficiency of removing methylene blue by photodegradation in rubber composite cement mortar with modified rubber after 12 hours of ultraviolet light irradiation reaches 96.6%.

[0025] The UV degradation curves of methylene blue show that the removal efficiency of the rubber-coated cement mortar with modified rubber was significantly increased by 200% compared to the unmodified rubber-coated cement mortar. This indicates that the modified rubber-coated cement mortar with modified waste tire rubber greatly enhances its photocatalytic performance.

[0026] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.

Claims

1. A method for preparing modified waste tire rubber, characterized in that, Includes the following steps: (1) Add waste tire rubber to an aqueous tannic acid solution and mix. Adjust the pH of the resulting mixture with an alkaline solution to obtain a pre-reaction solution; the waste tire rubber is in powder form. (2) Add titanium dioxide to the pre-reaction solution and react. After the reaction is completed, a reaction mixture is obtained. (3) The reaction mixture is filtered to obtain a filter cake, which is then washed and dried to obtain modified waste tire rubber.

2. The method according to claim 1, characterized in that: The mass ratio of the waste tire rubber, tannic acid, and titanium dioxide is 20:1:1~2.

3. The method according to claim 1, characterized in that: In step (1), the concentration of the tannic acid aqueous solution is 5~10g / L.

4. The method according to claim 1, characterized in that: In step (1), the pH of the mixture is adjusted to 8.0 ± 0.

2.

5. The method according to claim 1, characterized in that: In step (1), the alkaline solution is an aqueous solution of sodium hydroxide or potassium hydroxide, and the concentration of the alkaline solution is 0.1~0.5 mol / L.

6. The method according to claim 1, characterized in that: In step (2), the particle size of the titanium dioxide is <100nm.

7. The method according to claim 1, characterized in that: In step (2), the reaction is carried out at room temperature for 12-16 hours.

8. A modified waste tire rubber, characterized in that: It is prepared by the method described in any one of claims 1 to 7.

9. An application of the modified waste tire rubber as described in claim 8, characterized in that: Modified waste tire rubber, fine aggregate, and cement are mixed to prepare modified rubber composite cement mortar.