A polycarbonate composition, its preparation and use
By combining HIPS resin with a specific butadiene content with a composite toughening agent, the problem of improving the flexural strength and modulus of polycarbonate materials while maintaining toughness and flame retardancy has been solved, thus achieving the high-performance requirements of polycarbonate compositions in applications such as new energy vehicle components.
Patent Information
- Application Number
- CN202311579642.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-24
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-24
AI Technical Summary
While maintaining good toughness, existing polycarbonate materials are difficult to simultaneously possess good thin-wall flame retardancy, flexural strength, and flexural modulus. This is especially true in applications for new energy vehicle components, where it is difficult to achieve flame retardancy of V-0 (1.5mm), flexural strength of over 80MPa, and flexural modulus of over 2000MPa.
A polycarbonate composition is prepared by combining HIPS resin with a specific butadiene content with a specific composite toughening agent, including maleic anhydride-grafted SEBS and MBS or ABS, and adding an appropriate amount of flame retardant. The polycarbonate composition is prepared by melt extrusion.
The polycarbonate composition achieves V-0 (1.5 mm) flame retardancy while maintaining good notched impact strength, and has a flexural strength of over 80 MPa and a flexural modulus of over 2000 MPa.
Smart Images

Figure BDA0004568008820000051 
Figure BDA0004568008820000061 
Figure BDA0004568008820000062
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer material modification technology, and more specifically, to a polycarbonate composition, its preparation method, and its application. Background Technology
[0002] Polycarbonate (PC) is a thermoplastic engineering plastic with excellent overall performance, exhibiting superior transparency and flame retardancy, and thus having a wide range of applications. Current technology often blends polycarbonate with acrylonitrile-butadiene-styrene copolymer resin (ABS) to obtain good processing properties. However, polycarbonate molecules have high rigidity, and to meet application requirements, impact modifiers such as MBS and silicone-based toughening agents are generally added to improve toughness.
[0003] To further expand the application scenarios of polycarbonate materials in consumer electronics wearable devices, printer housings, and new energy vehicle components, polycarbonate materials are required to have good flame retardant properties, especially thin-walled flame retardant properties, requiring a V-0 (1.5mm) rating. However, if the amount of impact modifier used is too large, it is difficult to achieve a V-0 (1.5mm) flame retardant rating for polycarbonate materials.
[0004] In addition, when polycarbonate materials are used in new energy vehicle components, they are required to have good flexural strength and flexural modulus to ensure the deformation resistance and rigidity of the components. Currently, the flexural strength is required to be at least 80MPa and the flexural modulus to be at least 2000MPa.
[0005] Therefore, how to ensure excellent toughness while giving polycarbonate materials good thin-wall flame retardant properties, as well as good flexural strength and flexural modulus, is one of the problems that need to be solved in the field of polycarbonate materials. Summary of the Invention
[0006] The primary objective of this invention is to overcome the problems of current polycarbonate materials, which cannot simultaneously achieve good toughness and good thin-walled flame retardancy (V-0 (1.5 mm)) and have poor flexural strength and flexural modulus, and to provide a polycarbonate composition. The polycarbonate composition of this invention has good flexural strength and flexural modulus, and achieves V-0 (1.5 mm) flame retardancy while maintaining good notched impact strength.
[0007] A further object of the present invention is to provide a method for preparing the above-described polycarbonate composition.
[0008] A further object of the present invention is to provide the above-described polycarbonate composition for use in the manufacture of wearable devices for consumer electronics, printer housings, or components for new energy vehicles.
[0009] The above-mentioned objective of the present invention is achieved through the following technical solution:
[0010] A polycarbonate composition comprising the following components in parts by weight:
[0011] 62-80 parts of PC resin
[0012] 8-14 parts flame retardant
[0013] 8-18 parts of HIPS resin
[0014] 4-12 parts of composite toughening agent,
[0015] Anti-dripping agent 0.2-1 part;
[0016] The butadiene content of the HIPS resin is 17-26 wt%; the composite toughening agent includes a first toughening agent and a second toughening agent in a mass ratio of (4-1):1; the first toughening agent is at least one of SBS, SEBS or maleic anhydride-grafted SEBS, and the second toughening agent is at least one of MBS or ABS.
[0017] Through extensive research, the inventors of this invention discovered that by adding specific toughening agents (a combination of a first toughening agent and a second toughening agent) and HIPS resin with a specific butadiene content, the resulting polycarbonate composition exhibits excellent thin-wall flame retardant properties (V-0, 1.5 mm) while maintaining good notched impact strength. The reason for this is likely that HIPS with a specific butadiene content significantly improves impact resistance. However, directly adding HIPS resin to PC resin does not significantly enhance impact resistance. Adding a specific composite toughening agent to HIPS resin improves the dispersibility and compatibility of the HIPS resin, thereby enhancing the thin-wall flame retardant properties of the polycarbonate composition while maintaining good toughness (notched impact strength). Specifically, the polycarbonate composition of this invention achieves a notched impact strength of over 500 J / m, and its flame retardant properties reach V-0 (1.5 mm).
[0018] Furthermore, the polycarbonate composition of the present invention, through the combination of its components, also has good flexural strength and flexural modulus. Specifically, the flexural strength can reach more than 80 MPa and the flexural modulus can reach more than 2000 MPa.
[0019] That is, the polycarbonate composition of the present invention has good flexural strength and flexural modulus, and can achieve V-0 (1.5mm) flame retardant performance while maintaining good notched impact strength.
[0020] In the polycarbonate composition of the present invention, the content of PC resin is not less than 55 wt%.
[0021] Optionally, the number-average molecular weight of the PC resin is 17,000 to 45,000.
[0022] Preferably, the number average molecular weight of the PC resin is 23,000 to 28,000. Within this number average molecular weight range, the resulting polycarbonate composition has higher notched impact strength.
[0023] In this invention, the number-average molecular weight of PC resin can be determined by the GPC method.
[0024] Preferably, the butadiene content of the HIPS resin is 18.4 to 25 wt%, within which the polycarbonate composition exhibits better flexural modulus and notched impact strength.
[0025] Preferably, the average rubber particle size of the HIPS resin is 0.8 to 2.5 μm.
[0026] More preferably, the average rubber particle size of the HIPS resin is 2.0 to 2.5 μm.
[0027] In this invention, the average rubber particle size of the HIPS resin can be measured by transmission electron microscopy.
[0028] Preferably, the first toughening agent is maleic anhydride-grafted SEBS.
[0029] Using maleic anhydride-grafted SEBS results in polycarbonate compositions with higher notched impact strength, as well as higher flexural strength and flexural modulus.
[0030] Preferably, the second toughening agent is ABS.
[0031] Using ABS results in a polycarbonate composition with higher notched impact strength.
[0032] Preferably, the flame retardant is a phosphorus-containing flame retardant, which is at least one of bisphenol A (diphenyl phosphate), resorcinol (diphenyl phosphate), or phosphazene flame retardant.
[0033] More preferably, the phosphazene flame retardant is a phosphazene flame retardant. Using a phosphazene flame retardant results in a polycarbonate composition with higher notched impact strength.
[0034] More preferably, the phosphazene flame retardant is at least one of polyalkoxyphosphazene flame retardant, polyaryloxyphosphazene flame retardant, or cyclic tripolyphosphazene polymer.
[0035] Preferably, the polycarbonate composition further includes 0.4 to 1 part of other additives.
[0036] Optionally, the other additives include, but are not limited to, antioxidants, lubricants, or anti-dripping agents.
[0037] Optionally, the antioxidants include, but are not limited to, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphate, tris(2,4-di-tert-butylphenyl) phosphite, or pentaerythritol tetra(3-lauryl thiopropionate).
[0038] Optionally, the lubricant includes, but is not limited to, fatty acid metal salts, ester lubricants, amide lubricants, paraffin wax, lignite wax, or silicone.
[0039] Optionally, the fatty acid metal salt lubricant includes, but is not limited to, magnesium stearate lubricant or sodium stearate lubricant.
[0040] Optionally, the ester lubricant includes, but is not limited to, pentaerythritol tetrastearate, fatty acid esters, etc.
[0041] Optionally, the amide lubricant includes, but is not limited to, oleamide lubricants, amide soap lubricants, or stearyl erucamide lubricants.
[0042] Optionally, the anti-dripping agent includes, but is not limited to, polytetrafluoroethylene.
[0043] Preferably, the polycarbonate composition comprises the following components in parts by weight:
[0044] 65-72 parts of PC resin
[0045] 11-13 parts flame retardant
[0046] 10-13 parts of HIPS resin
[0047] 7-9 parts of composite toughening agent,
[0048] Anti-dripping agent 0.2 to 1 part.
[0049] The preparation method of the above polycarbonate composition includes the following steps: mixing the components and melt extruding to obtain the polycarbonate composition.
[0050] Preferably, the temperature of the melt extrusion is 210–230°C.
[0051] The above-mentioned polycarbonate composition is also within the scope of protection of this invention when used in the manufacture of wearable devices for consumer electronics, printer housings, or new energy vehicle components.
[0052] Compared with the prior art, the beneficial effects of the present invention are:
[0053] The polycarbonate composition of the present invention has good flexural strength and flexural modulus, and can achieve V-0 (1.5 mm) flame retardant performance while maintaining good notched impact strength. Detailed Implementation
[0054] To more clearly and completely describe the technical solution of the present invention, the present invention will be further described in detail below through specific embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the present invention. Various changes can be made within the scope of the claims of the present invention.
[0055] The reagents used in the various embodiments and comparative examples of this invention are described below:
[0056] PC resin #1: Number average molecular weight is 28000, S-2000F, Mitsubishi;
[0057] PC resin #2: Number average molecular weight is 23000, S-3000F, Mitsubishi;
[0058] PC resin #3: Number average molecular weight 40,000, K-1000F, Mitsubishi;
[0059] HIPS resin 1#: PS 350K, Guoheng, Taiwan, China, with an average rubber particle size of 2.0-2.5μm and a butadiene content of 18.4wt%.
[0060] HIPS resin #2: PH-888G, Zhenjiang Qimei, with an average rubber particle size of 1.0-1.2μm and a butadiene content of 24.1wt%.
[0061] HIPS Resin 3#: HIPS 825G, Formosa Plastics (Ningbo) Co., Ltd., with an average rubber particle size of 0.9-1.1μm and a butadiene content of 15%;
[0062] GPPS resin: 123P, Shanghai SECCO, butadiene-free;
[0063] First toughening agent #1: SEBS grafted maleic anhydride, SEBS FG1901 GT, Kraton, USA;
[0064] First toughening agent #2: SEBS, YH-501, Baling Petrochemical;
[0065] First toughening agent #3: SBS, YH-792, Baling Petrochemical;
[0066] Second toughening agent 1#: MBS, M-505, Formosa Plastics Group, China;
[0067] Second toughening agent #2: ABS, ABS 8434, Gaoqiao Petrochemical;
[0068] Common toughening agent #1: POE grafted with maleic anhydride, N493, DuPont, USA;
[0069] The formulations of composite toughening agents 1 to 11# are shown in Table 1.
[0070] Table 1. Formulation of composite toughening agent (parts by weight)
[0071]
[0072] Phosphorus-based flame retardant #1: Phosphate ester flame retardant, FP-600, from Japan's Adico;
[0073] Phosphorus-based flame retardant #2: Phosphazene flame retardant, SPB-100, Otsuka, Japan;
[0074] Anti-dripping agent: TS 30A, commercially available;
[0075] Other additives: Lubricant, LOXIOL P861 / 3.5, commercially available.
[0076] Unless otherwise specified, all components (e.g., anti-dripping agents, other additives) used in each parallel embodiment and comparative example are the same commercially available products.
[0077] The polycarbonate compositions provided in the embodiments and comparative examples of the present invention were subjected to performance testing according to the following test methods:
[0078] (1) Bending strength: tested on a Zwick electronic universal testing machine in accordance with standard ASTM D790-2003;
[0079] (2) Flexural modulus: Tested on a Zwick electronic universal testing machine in accordance with standard ASTM D790-2003;
[0080] (3) Notched impact strength of cantilever beam: tested on a Zwick electronic universal testing machine in accordance with standard ASTM D256-2010;
[0081] (4) Flame retardant rating: According to standard UL94-2021, the thickness is selected as 1.5mm during the test.
[0082] The polycarbonate compositions of the various embodiments of the present invention were prepared by the following methods:
[0083] According to the formulas in Tables 2-3, weigh out each component; then mix the components, melt extrude (the temperatures of each zone of the extruder are: zone 1 210℃, zone 2 220℃, zone 3 220℃, zone 4 220℃, zone 5 230℃, zone 6 230℃, zone 7 230℃, zone 8 230℃, zone 9 230℃, zone 10 230℃, zone 11 230℃, main machine speed 450 rpm), granulate, and the polycarbonate composition is obtained.
[0084] Examples 1-15
[0085] Examples 1-15 provide a series of polycarbonate compositions, the formulations of which are shown in Tables 2 and 3.
[0086] 2. Formulations (parts by weight) of Examples 1-9
[0087]
[0088] Table 3. Formulations (parts by weight) for Examples 10-15
[0089]
[0090]
[0091] Comparative Example 1
[0092] This comparative example provides a polycarbonate composition whose preparation method and formulation are basically the same as those in Example 1, except that HIPS resin 1# is replaced with HIPS resin 3#.
[0093] Comparative Example 2
[0094] This comparative example provides a polycarbonate composition whose preparation method and formulation are basically the same as those in Example 1, except that HIPS resin 1# is replaced with GPPS resin.
[0095] Comparative Example 3
[0096] This comparative example provides a polycarbonate composition whose preparation method and formulation are basically the same as those in Example 1, except that composite toughening agent 1# is replaced with composite toughening agent 8#.
[0097] Comparative Example 4
[0098] This comparative example provides a polycarbonate composition whose preparation method and formulation are basically the same as those in Example 1, except that composite toughening agent 1# is replaced with composite toughening agent 9#.
[0099] Comparative Example 5
[0100] This comparative example provides a polycarbonate composition whose preparation method and formulation are basically the same as those in Example 1, except that composite toughening agent 1# is replaced with composite toughening agent 10#.
[0101] Comparative Example 6
[0102] This comparative example provides a polycarbonate composition whose preparation method and formulation are basically the same as those in Example 1, except that composite toughening agent 1# is replaced with composite toughening agent 11#.
[0103] Comparative Example 7
[0104] This comparative example provides a polycarbonate composition whose preparation method and formulation are basically the same as those in Example 1, except that composite toughening agent 1# is replaced with ordinary toughening agent 1#.
[0105] Comparative Example 8
[0106] This comparative example provides a polycarbonate composition whose preparation method and formulation are basically the same as those in Example 1, except that composite toughening agent 1# is replaced with first toughening agent 1#.
[0107] Comparative Example 9
[0108] This comparative example provides a polycarbonate composition whose preparation method and formulation are basically the same as those in Example 1, except that composite toughening agent 1# is replaced with second toughening agent 1#.
[0109] The properties of the polycarbonate compositions of each embodiment and comparative example were determined according to the test methods mentioned above, and the test results are shown in Table 4.
[0110] Table 4. Performance test results of the polycarbonate compositions of each example and comparative example.
[0111]
[0112]
[0113] As can be seen from Table 4:
[0114] The polycarbonate compositions of Examples 1-15 exhibit notched impact strengths of 500 J / m or higher and flame retardant properties of V-0 (1.5 mm), indicating that the polycarbonate compositions of the present invention can achieve V-0 (1.5 mm) flame retardant properties while maintaining good notched impact strength. Furthermore, the polycarbonate compositions of Examples 1-15 also possess good flexural strength and flexural modulus, with a strength of 80 MPa or higher and a flexural modulus of 2000 MPa or higher.
[0115] In Comparative Example 1, the ethylene content of the HIPS resin was unsuitable, resulting in a polycarbonate composition with low notched impact strength. Comparative Example 2, which used GPPS resin instead of HIPS resin, also resulted in a polycarbonate composition with low notched impact strength. Comparative Examples 3 and 4 used composite toughening agents 8# and 9#, respectively. However, the mass ratio of the first and second toughening agents in these agents was unsuitable, leading to a polycarbonate composition that failed to achieve both good notched impact strength and flame retardant properties. Comparative Examples 5 and 6 used composite toughening agents 10# and 11#, respectively. The types of the first or second toughening agents used in both examples were unsuitable, resulting in a polycarbonate composition that failed to achieve both good notched impact strength and flame retardant properties. Comparative Example 7 did not use a composite toughening agent but instead used POE grafted with maleic anhydride, resulting in a polycarbonate composition with poor notched impact strength and flame retardant properties. Comparative Examples 8 and 9 did not use composite toughening agents, but instead used single toughening agents. Both had poor notched impact strength, with Comparative Example 9 also having poor flame retardant properties.
[0116] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. Those skilled in the art can make other variations or modifications based on the above description. It is neither necessary nor possible to exhaustively describe all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.
Claims
1. A polycarbonate composition, characterized in that, The components include the following parts by weight: The butadiene content of the HIPS resin is 17-26 wt%; the composite toughening agent includes a first toughening agent and a second toughening agent in a mass ratio of (4-1):1; the first toughening agent is at least one of SBS, SEBS or maleic anhydride-grafted SEBS, and the second toughening agent is at least one of MBS or ABS.
2. The polycarbonate composition according to claim 1, characterized in that, The number average molecular weight of the PC resin is 17,000 to 45,000.
3. The polycarbonate composition according to claim 1, characterized in that, The average rubber particle size of the HIPS resin is 0.8–2.5 μm.
4. The polycarbonate composition according to claim 1, characterized in that, The first toughening agent is maleic anhydride-grafted SEBS.
5. The polycarbonate composition according to claim 1, characterized in that, The second toughening agent is ABS.
6. The polycarbonate composition according to claim 1, characterized in that, The flame retardant is a phosphorus-containing flame retardant, which is at least one of bisphenol A (diphenyl phosphate), resorcinol (diphenyl phosphate), and phosphazene flame retardant.
7. The polycarbonate composition according to claim 1, characterized in that, The polycarbonate composition also includes 0.4 to 1 part of other additives.
8. The polycarbonate composition according to claim 1, characterized in that, The polycarbonate composition comprises the following components in parts by weight:
9. A method for preparing the polycarbonate composition according to any one of claims 1 to 8, characterized in that, The process includes the following steps: mixing the components and melting and extruding them to obtain the polycarbonate composition.
10. The polycarbonate composition according to any one of claims 1 to 8 is used in the preparation of wearable devices for consumer electronics, printer housings, or components for new energy vehicles.
Citation Information
Patent Citations
Case material for liquid crystal display television capacitors and preparation method of case material
CN107057258A
Flame retardant polycarbonate resin composition
CN111094452A