A smelting method for improving the surface quality of titanium alloy primary ingot
By controlling the melting parameters and vacuum protection cooling of the vacuum consumable arc furnace, the problem of black scale on the surface of primary titanium alloy ingots was solved, the ingot quality and the safety of the welding process were improved, and efficient titanium alloy melting was achieved.
Patent Information
- Application Number
- CN202311389171.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-25
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-10-25
AI Technical Summary
The surface of existing titanium alloy primary ingots has a large amount of black scale, which is prone to cracking and peeling, affecting the quality of the ingot and the process requirements of subsequent welding.
By controlling the melting parameters of the vacuum consumable arc furnace, such as vacuum degree, leakage rate, welding current and voltage, melting current and voltage, and combined with vacuum protection cooling, high-quality titanium alloy primary ingots can be prepared.
It significantly reduced black skin cracking and peeling, improved the yield and appearance quality of finished ingots, reduced the risk of secondary smelting, and improved the safety and economic benefits of the smelting process.
Smart Images

Figure CN117512368B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of non-ferrous metal processing technology, and specifically relates to a smelting method for improving the surface quality of titanium alloy primary ingots. Background Technology
[0002] As is well known, titanium is an important structural metal developed in the 1950s. Titanium alloys are alloys composed of titanium as the base and other elements. Due to its high strength, corrosion resistance, good low-temperature performance, heat resistance and high thermal strength, titanium and titanium alloys have become very important structural materials in many industries, such as aerospace, medical and automotive industries. At the same time, they have broad application prospects in metallurgy, petrochemicals, electronic light sources and machinery manufacturing.
[0003] Currently, the main methods for melting titanium alloys include five types: vacuum arc remelting (VAR), non-arsenic vacuum arc remelting (NC), cold hearth melting (CHM), cold crucible melting (CCM), and electroslag remelting (ESR). Due to its low power consumption, fast melting speed, and good quality reproducibility, the VAR method produces ingots with excellent crystalline structure and uniform chemical composition, making it the mainstream technology for titanium alloy ingot preparation. The VAR process typically involves two or three melting stages.
[0004] In the primary melting process, the consumable electrode is composed of electrode blocks pressed from a mixture of sponge titanium and intermediate alloy, forming a physically bonded block. Therefore, during primary melting, impurities in the electrode blocks continuously volatilize upon heating. Under the influence of the arc-stabilizing stirring magnetic field, floating matter and impurities in the molten pool condense and precipitate along the inner wall of the water-cooled copper crystallizer, forming a black surface layer. Consequently, if multiple control parameters are not properly coordinated, the resulting titanium alloy primary ingot will have a large amount of cracked black surface layer. This black surface layer has a high impurity content and is easily detached after heating and cooling. During subsequent secondary melting, it may fall into the molten pool, affecting the ingot quality. Furthermore, the detached surface black surface layer severely affects the original dimensions of the ingot. Later, during vacuum plasma welding, when two or more primary ingots are placed on the fixture, gaps exist at the connection points, preventing tight bonding or ensuring the straightness of the consumable electrode meets process and furnace loading requirements after welding.
[0005] In view of this, the present invention is hereby proposed. Summary of the Invention
[0006] To achieve the above objectives, the present invention provides the following technical solution:
[0007] A smelting method for improving the surface quality of titanium alloy primary ingots specifically includes the following steps:
[0008] Step 1: Determine the crucible specifications required for one melting operation based on the melting capacity and feed amount of the vacuum consumable arc furnace.
[0009] Step 2: Determine the component ratio of the ingot to be fed based on the chemical composition of the target grade ingot;
[0010] Step 3: Calculate and prepare the corresponding raw materials according to the component ratio determined in Step 2, and use a V-type mixer to mix the raw materials evenly to form a mixture;
[0011] Step 4: Use a hydraulic press to press the mixture obtained in step 3 into electrode blocks that match the crucible specifications determined in step 1.
[0012] Step 5: Place the electrode blocks obtained in Step 4 in the designated fixture according to their serial numbers, and perform flatness treatment on each electrode block and clean up the debris stuck between the electrode blocks or between the electrode blocks and the material rack. Then, use the fixture to fix the multiple electrode blocks that have been placed. Then, weld the multiple electrode blocks into consumable electrodes in the vacuum plasma welding box. After cooling and taking them out of the furnace, clean the weld beads.
[0013] Step 6: Under the set parameters, the consumable electrode obtained in Step 5 is melted once in a vacuum consumable arc furnace. After the first melting is completed, the ingot is cooled for a period of time, and argon gas is introduced into the furnace cavity. Under the protection of argon gas, it is cooled to below 400°C and then taken out of the furnace to obtain the target titanium alloy primary ingot.
[0014] Furthermore, the mixing time in step 3 is set to 3 to 5 minutes.
[0015] Further, the specific process of pressing the electrode block in step 4 is as follows: the mixture obtained in step 3 is poured into the inner cavity of the mold matched with the hydraulic press, and the mixture is pressed into an electrode block according to the following pressing parameters: pressure is 21MPa~24MPa, holding time is 20s~25s, and upper mold moving speed is 0.06m / min~0.10m / min.
[0016] Furthermore, the parameters for welding the electrode block in the vacuum plasma welding box in step 5 are: vacuum degree ≤ 3.5 Pa, leakage rate ≤ 1 Pa / min, welding current 400 A~600 A, and welding voltage 50 V~70 V.
[0017] Furthermore, in step 6, the parameters for the self-consuming electrode to be melted once in a vacuum self-consuming electric arc furnace are as follows: melting current is 8KA~25KA, melting voltage is 28V~38V, arc stabilization current is DC 10A~25A, vacuum degree before melting is ≤1Pa, leakage rate is ≤1Pa / min, and vacuum is controlled at 1Pa~5Pa during melting.
[0018] Furthermore, in step 6, after the ingot is cooled for 1 to 2 hours after the first melting is completed, argon gas is introduced into the furnace cavity.
[0019] Furthermore, the straightness of the length direction of several titanium alloy ingots obtained by the smelting method after welding is ≤5mm / m.
[0020] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0021] The smelting method provided by this invention controls key smelting process parameters, including but not limited to vacuum degree, leakage rate, welding current and voltage, smelting current and voltage, arc stabilization current, and vacuum degree during smelting. Through the synergistic effect of these parameters, the final titanium alloy primary ingot significantly reduces the phenomenon of black skin cracking and peeling, avoids the risk of surface black skin forming inclusions during secondary smelting, and is conducive to increasing the yield of finished ingots and improving economic efficiency. At the same time, it can obtain titanium alloy primary ingots with excellent appearance quality and small dimensional differences. Furthermore, the straightness of the length direction of multiple titanium alloy primary ingots after welding is ≤5mm / m. Therefore, it reduces the risk of edge arcing between the electrode and crucible during secondary smelting and improves the safety of the vacuum consumable melting process. Attached Figure Description
[0022] The accompanying drawings are incorporated in and form part of this specification, and together with the description serve to explain the principles of the invention.
[0023] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] Figure 1 This is a flowchart of the smelting method of the present invention;
[0025] Figure 2 The image shows the morphology of a Φ570mm TA15 primary ingot prepared in Example 1 of this invention.
[0026] Figure 3 The image shows the morphology of the Φ570mm TC4 primary ingot prepared in Example 2 of this invention.
[0027] Figure 4 The image shows the morphology of the Φ450mm TA15 primary ingot prepared in Example 3 of this invention.
[0028] Figure 5 The image shows the appearance of the 450mm TC4 primary ingot prepared in Example 4 of this invention. Detailed Implementation
[0029] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numbers in different drawings denote the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Rather, they are merely examples consistent with some aspects of the invention as detailed in the appended claims.
[0030] To enable those skilled in the art to better understand the technical solutions of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments.
[0031] like Figure 1 As shown, the present invention provides a smelting method for improving the surface quality of titanium alloy primary ingots, characterized by comprising the following steps:
[0032] Step 1: Determine the crucible specifications required for one melting operation based on the melting capacity and feed amount of the vacuum consumable arc furnace.
[0033] Step 2: Determine the component ratio of the ingot to be fed based on the chemical composition of the target grade ingot;
[0034] Step 3: Calculate and prepare the corresponding raw materials according to the component ratio determined in Step 2, and pour all the raw materials into the V-type mixer for mixing. The mixing time is 3 to 5 minutes. After mixing evenly, a mixture is formed.
[0035] Step 4: Use a hydraulic press to press the mixture obtained in Step 3 into electrode blocks that match the crucible specifications determined in Step 1; specifically, pour the mixture obtained in Step 3 into the inner cavity of the mold matched with the hydraulic press, and press the mixture into electrode blocks according to the following pressing parameters: pressure 21MPa~24MPa, holding time 20s~25s, upper mold moving speed 0.06m / min~0.10m / min;
[0036] Step 5: Place the electrode blocks obtained in Step 4 in the designated fixture according to their serial numbers, and perform flatness treatment on each electrode block and clean up the debris stuck between the electrode blocks or between the electrode blocks and the material rack. Then, use the fixture to fix the multiple electrode blocks that have been placed. Then, weld the multiple electrode blocks into consumable electrodes in the vacuum plasma welding box. After cooling and taking them out of the furnace, clean the weld beads.
[0037] Specifically, the parameters for welding the electrode blocks in the vacuum plasma welding box are: vacuum degree ≤3.5Pa, leakage rate ≤1Pa / min, welding current 400A~600A, and welding voltage 50V~70V;
[0038] Step 6: Under set parameters, the consumable electrode obtained in Step 5 is subjected to a single melting process in a vacuum consumable arc furnace. The parameters for the single melting process are: melting current of 8KA to 25KA, melting voltage of 28V to 38V, arc stabilization current of DC 10A to 25A, vacuum degree ≤1Pa before melting, leakage rate ≤1Pa / min, and vacuum control of 1Pa to 5Pa during melting. This is because when the vacuum degree is less than 1Pa, the surface quality of the primary ingot deteriorates, with localized cracks and black scale, making it prone to moisture absorption when stored in the atmosphere, which can easily lead to defects such as porosity during subsequent melting. After the primary melting process, the ingot is cooled for 1 to 2 hours, and then argon gas is introduced into the furnace cavity. Under argon protection, it is cooled to below 400℃ before being removed from the furnace, thus obtaining the target titanium alloy primary ingot.
[0039] To further verify the effectiveness of the preparation method of the present invention, the inventors conducted the following specific experiments:
[0040] Example 1 (Preparation of TA15 primary ingot with a diameter of Φ570mm)
[0041] The preparation method in this embodiment specifically includes the following steps:
[0042] 1) Based on the melting capacity and melting process of the vacuum self-consuming electric arc furnace, the crucible size required for one melting is determined to be Φ570×2500mm.
[0043] 2) Determine the composition ratio of the TA15 ingot in this batch based on the chemical composition range of GB / T 3620.1-2019.
[0044] 3) Calculate and select the required raw materials based on the proportions determined in step 2, including sponge titanium, aluminum vanadium alloy, aluminum molybdenum alloy, aluminum briquettes, sponge zirconium, and titanium dioxide. Pour the weighed intermediate alloy and sponge titanium into a V-type mixer for mixing. After mixing for 4 minutes, a TA15 mixture is formed.
[0045] 4) Pour the TA15 mixture obtained in step 3) into the inner cavity of the Φ450mm mold of the hydraulic press, set the pressing pressure P = 23MPa, the holding time t = 23s, and the upper mold moving speed V = 0.08m / min, press the electrode block that matches the crucible size, with a size of Φ450×300mm, and mark it.
[0046] 5) Arrange the electrode blocks obtained in step 4) sequentially in the designated fixture. Use a hammer to adjust the position of the electrode blocks, knock off any burrs affecting the straightness of the electrode blocks, and clean up any debris stuck between the electrode blocks or between the electrode blocks and the material rack. The arranged electrode blocks should be flat, straight, and tightly fitted. Then, fix the upper fixture, tighten the bolts at both ends, and clamp the electrodes. Then, weld the arranged electrode blocks into a single consumable electrode in a vacuum plasma welding box. After cooling and removal from the furnace, clean off any weld beads. The welding parameters for the electrode blocks in the vacuum plasma welding box are: vacuum degree 2.8 Pa, leakage rate 0.8 Pa / min, welding current 600 A, and welding voltage 60 V.
[0047] 6) The consumable electrode obtained in step 5) is smelted once in a vacuum consumable arc furnace. The smelting current is 21 kA, the smelting voltage is 33 V, the arc stabilizing current is DC 19 A, the vacuum degree before melting is ≤1 Pa, the leakage rate is 0.53 Pa / min, and the vacuum during melting is maintained at 1.31~4.82 Pa. After the first smelting, the ingot is cooled for 1.5 h, and then argon gas is introduced into the furnace cavity. Under the protection of argon gas, it is cooled to 380 °C and then taken out of the furnace to obtain the target TA15 primary ingot.
[0048] The macroscopic morphology of the TA15 primary ingot obtained in Example 1 is as follows: Figure 2 As shown, the appearance quality is good, and there is no large amount of easily peeling black skin on the surface. At the same time, the straightness of the length direction of the two primary ingots after welding is 3mm / m, which fully meets the process requirements of secondary charging and smelting.
[0049] Example 2 (Preparation of TC4 primary ingot with a specification of Φ570mm)
[0050] The preparation method in this embodiment specifically includes the following steps:
[0051] 1) Based on the melting capacity and melting process of the vacuum self-consuming electric arc furnace, the crucible size required for one melting is determined to be Φ570×2500mm.
[0052] 2) Determine the composition ratio of the ingot to be fed in this batch based on the chemical composition range of TC4 ingot in GB / T 3620.1-2019.
[0053] 3) Calculate and select the required raw materials based on the proportions determined in step 2, including sponge titanium, aluminum vanadium alloy, aluminum briquettes, and titanium dioxide. Pour the weighed intermediate alloy and sponge titanium into a V-type mixer for mixing. After mixing for 5 minutes, a TA15 mixture is formed.
[0054] 4) Pour the TA15 mixture obtained in step 3) into the inner cavity of the Φ450mm mold of the hydraulic press, set the pressing pressure P = 23MPa, the holding time t = 20s, and the upper mold moving speed V = 0.10m / min, press the electrode block that matches the crucible size, with a size of Φ450×300mm, and mark it.
[0055] 5) Arrange the electrode blocks obtained in step 4) sequentially in the designated fixture. Use a hammer to adjust the position of the electrode blocks, knock off any burrs affecting the straightness of the electrode blocks, and clean up any debris stuck between the electrode blocks or between the electrode blocks and the material rack. The arranged electrode blocks should be flat, straight, and tightly fitted. Then, fix the upper fixture, tighten the bolts at both ends, and clamp the electrodes. Then, weld the arranged electrode blocks into a single consumable electrode in a vacuum plasma welding box. After cooling and removal from the furnace, clean off any weld beads. The welding parameters for the electrode blocks in the vacuum plasma welding box are: vacuum degree 2.5 Pa, leakage rate 0.51 Pa / min, welding current 550 A, and welding voltage 70 V.
[0056] 6) The consumable electrode obtained in step 5) is melted once in a vacuum consumable arc furnace. The melting current is 23KA, the melting voltage is 35V, the arc stabilizing current is DC 25A, the vacuum degree before melting is ≤0.74Pa, the leakage rate is ≤0.85Pa / min, and the vacuum during melting is maintained at 1.28~4.86Pa. After the first melting is completed, the ingot is cooled for 2 hours, and then argon gas is introduced into the furnace cavity. Under the protection of argon gas, it is cooled to 360℃ and then taken out of the furnace to obtain the target TC4 primary ingot.
[0057] The macroscopic morphology of the TC4 primary ingot obtained in Example 2 is as follows: Figure 3 As shown, the appearance quality is good, and there is no large amount of easily peeling black skin on the surface. At the same time, the straightness of the length direction of the two primary ingots after welding is 4mm / m, which fully meets the process requirements of secondary charging and smelting.
[0058] Example 3 (Preparation of TA15 primary ingot with a specification of Φ450mm)
[0059] The preparation method in this embodiment specifically includes the following steps:
[0060] 1) Based on the melting capacity and melting process of the vacuum self-consuming electric arc furnace, the crucible size required for one melting is determined to be Φ450×2200mm.
[0061] 2) Determine the composition ratio of the TA15 ingot in this batch based on the chemical composition range of GB / T 3620.1-2019.
[0062] 3) Calculate and select the required raw materials based on the proportions determined in step 2, including sponge titanium, aluminum vanadium alloy, aluminum molybdenum alloy, aluminum briquettes, sponge zirconium, and titanium dioxide. Pour the weighed intermediate alloy and sponge titanium into a V-type mixer for mixing. After mixing for 3 minutes, a TA15 mixture is formed.
[0063] 4) Pour the TA15 mixture obtained in step 3) into the inner cavity of the Φ360mm mold of the hydraulic press, set the pressing pressure P=22MPa, the holding time t=25s, and the upper mold moving speed V=0.06m / min, press the electrode block that matches the crucible size, with a size of Φ360×400mm, and mark it.
[0064] 5) Arrange the electrode blocks obtained in step 4) sequentially in the designated fixture. Use a hammer to adjust the position of the electrode blocks, knock off any burrs affecting the straightness of the electrode blocks, and clean up any debris stuck between the electrode blocks or between the electrode blocks and the material rack. The arranged electrode blocks should be flat, straight, and tightly fitted. Then, fix the upper fixture, tighten the bolts at both ends, and clamp the electrodes. Then, weld the arranged electrode blocks into a single consumable electrode in a vacuum plasma welding box. After cooling and removal from the furnace, clean off any weld beads. The welding parameters for the electrode blocks in the vacuum plasma welding box are: vacuum degree 1.98 Pa, leakage rate ≤0.75 Pa / min, welding current 500 A, and welding voltage 55 V.
[0065] 6) The consumable electrode obtained in step 5) is melted once in a vacuum consumable arc furnace. The melting current is 16 kA, the melting voltage is 28 V, the arc stabilizing current is DC 18 A, the vacuum degree before melting is 0.75 Pa, the leakage rate is ≤0.91 Pa / min, and the vacuum during melting is maintained at 1.35~4.56 Pa. After the first melting is completed, the ingot is cooled for 1 hour, and then argon gas is introduced into the furnace cavity. Under the protection of argon gas, it is cooled to 386°C and then taken out of the furnace to obtain the target TA15 primary ingot.
[0066] The macroscopic morphology of the TA15 primary ingot obtained in Example 3 is as follows: Figure 4 As shown, the appearance quality is good, and there is no large amount of easily peeling black skin on the surface. At the same time, the straightness of the length direction of the two primary ingots after welding is 3mm / m, which fully meets the process requirements of secondary charging and smelting.
[0067] Example 4 (Preparation of a TC4 primary ingot with a diameter of Φ450mm)
[0068] The preparation method in this embodiment specifically includes the following steps:
[0069] 1) Based on the melting capacity and melting process of the vacuum self-consuming electric arc furnace, the crucible size required for one melting is determined to be Φ450×2200mm.
[0070] 2) Determine the composition ratio of the ingot to be fed in this batch based on the chemical composition range of TC4 ingot in GB / T 3620.1-2019.
[0071] 3) Calculate and select the required raw materials based on the proportions determined in step 2, including sponge titanium, aluminum vanadium alloy, aluminum briquettes, and titanium dioxide. Pour the weighed intermediate alloy and sponge titanium into a V-type mixer for mixing. After mixing for 5 minutes, TC4 mixture is formed.
[0072] 4) Pour the TA15 mixture obtained in step 3) into the inner cavity of the Φ360mm mold of the hydraulic press, set the pressing pressure P = 22MPa, the holding time t = 22s, and the upper mold moving speed V = 0.09m / min, press the electrode block that matches the crucible size, with a size of Φ360×400mm, and mark it.
[0073] 5) Arrange the electrode blocks obtained in step 4) sequentially in the designated fixture. Use a hammer to adjust the position of the electrode blocks, knock off any burrs affecting the straightness of the electrode blocks, and clean up any debris stuck between the electrode blocks or between the electrode blocks and the material rack. The arranged electrode blocks should be flat, straight, and tightly fitted. Then, fix the upper fixture, tighten the bolts at both ends, and clamp the electrodes. Then, weld the arranged electrode blocks into a single consumable electrode in a vacuum plasma welding box. After cooling and removal from the furnace, clean off any weld beads. The welding parameters for the electrode blocks in the vacuum plasma welding box are: vacuum degree 1.86 Pa, leakage rate ≤0.84 Pa / min, welding current 480 A, and welding voltage 63 V.
[0074] 6) The consumable electrode obtained in step 5) is smelted once in a vacuum consumable arc furnace. The smelting current is 12KA, the smelting voltage is 30V, the arc stabilizing current is DC 15A, the vacuum degree before melting is 0.63Pa, the leakage rate is 0.57Pa / min, and the vacuum during melting is maintained at 1.48~4.76Pa. After the first smelting, the ingot is cooled for 1 hour, and then argon gas is introduced into the furnace cavity. Under the protection of argon gas, it is cooled to below 400℃ and then taken out of the furnace to obtain the target TC4 primary ingot.
[0075] The macroscopic morphology of the TC4 primary ingot obtained in Example 4 is as follows: Figure 5 As shown, the appearance quality is good, and there is no large amount of easily peeling black skin on the surface. At the same time, the straightness of the length direction of the two primary ingots after welding is 5mm / m, which fully meets the process requirements of secondary charging and smelting.
[0076] In summary, this invention employs a vacuum consumable melting method to prepare primary titanium alloy ingots. By controlling various process parameters during melting, particularly the coordinated operation of vacuum level, welding current and voltage, and melting current and voltage, specifically, after the primary ingot melting current reaches stability and the molten pool is intact, the diffusion pump is manually shut off. During melting, a mechanical pump and a Roots pump are used for evacuation, maintaining the vacuum level between 1 Pa and 5 Pa until the melting is complete. This not only reduces the electrical energy consumption in titanium alloy melting and improves economic efficiency but also yields excellent appearance quality of primary titanium alloy ingots.
[0077] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention.
[0078] It should be understood that the present invention is not limited to the content already described above, and various modifications and changes can be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A smelting method for improving the surface quality of a primary titanium alloy ingot, characterized in that, Specifically, the following steps are included: Step 1: Determine the crucible specifications required for one melting operation based on the melting capacity and feed amount of the vacuum consumable arc furnace. Step 2: Determine the component ratio of the ingot to be fed based on the chemical composition of the target grade ingot; Step 3: Calculate and prepare the corresponding raw materials according to the component ratio determined in Step 2, and use a V-type mixer to mix the raw materials evenly to form a mixture; Step 4: Use a hydraulic press to press the mixture obtained in step 3 into electrode blocks that match the crucible specifications determined in step 1. Step 5: Place the electrode blocks obtained in Step 4 in the designated fixture according to their serial numbers, and perform flatness treatment on each electrode block and clean up the debris stuck between the electrode blocks or between the electrode blocks and the material rack. Then, use the fixture to fix the multiple electrode blocks that have been placed. Then, weld the multiple electrode blocks into consumable electrodes in the vacuum plasma welding box. After cooling and taking them out of the furnace, clean the weld beads. Step 6: Under the set parameters, the consumable electrode obtained in step 5 is melted once in a vacuum consumable arc furnace. After the first melting is completed, the ingot is cooled for a period of time, and then argon gas is introduced into the furnace cavity. Under the protection of argon gas, it is cooled to below 400°C and then taken out of the furnace to obtain the target titanium alloy primary ingot. In step 6, the parameters for the consumable electrode to be melted once in a vacuum consumable arc furnace are as follows: melting current is 8kA~25kA, melting voltage is 28V~38V, arc stabilization current is DC 10A~25A, vacuum degree before melting is ≤1Pa, leakage rate is ≤1Pa / min, and vacuum degree is controlled at 1Pa~5Pa during melting. After the first melting in step 6 is completed, the ingot is cooled for 1 to 2 hours before argon gas is introduced into the furnace cavity.
2. The smelting method for improving the surface quality of titanium alloy primary ingots according to claim 1, characterized in that, In step 3, the mixing time is set to 3 to 5 minutes.
3. The smelting method for improving the surface quality of titanium alloy primary ingots according to claim 1, characterized in that, The specific process of pressing the electrode block in step 4 is as follows: the mixture obtained in step 3 is poured into the inner cavity of the mold matched with the hydraulic press, and the mixture is pressed into an electrode block according to the following pressing parameters: pressure is 21MPa~24MPa, holding time is 20s~25s, and upper mold moving speed is 0.06m / min~0.10m / min.
4. The smelting method for improving the surface quality of titanium alloy primary ingots according to claim 1, characterized in that, In step 5, the parameters for welding the electrode block in the vacuum plasma welding box are: vacuum degree ≤ 3.5 Pa, leakage rate ≤ 1 Pa / min, welding current 400 A~600 A, and welding voltage 50 V~70 V.
5. The smelting method for improving the surface quality of titanium alloy primary ingots according to any one of claims 1 to 4, characterized in that, The straightness of the length direction of several titanium alloy ingots obtained by the smelting method after welding is ≤5mm / m.
Citation Information
Patent Citations
Treatment method for reducing oxygen content of titanium alloy cast ingot
CN113025831A
Vacuum consumable melting method for high-Mo-content Ti-Mo alloy homogeneous cast ingot
CN113278812A