A high surface high hole expanding steel and a method of manufacturing the same
By rationally designing the chemical composition and hot rolling process, a high-expansion steel with a high proportion of ferrite + bainite structure is formed, which solves the problems of low expansion rate and poor surface quality of existing high-expansion steel, and achieves steel properties with high surface quality and high expansion rate, which is suitable for forming automotive parts.
Patent Information
- Application Number
- CN202210897817.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-07-28
AI Technical Summary
The existing high-expansion steel has an insufficient expansion rate and poor surface quality, making it difficult to meet the requirements of complex forming of automotive parts.
By rationally designing the chemical composition and hot rolling process, controlling the content of elements such as C, Si, Mn, and Al, and optimizing the hot rolling process parameters, a high proportion of ferrite + bainite structure is formed, ensuring high surface quality and high porosity of the steel.
It achieves a yield strength Rel≥305MPa, tensile strength Rm≥440MPa, elongation A≥34%, and hole expansion rate λ≥90%, meeting the performance requirements of automotive chassis and complex stamped parts, and has good application prospects.
Smart Images

Figure CN117512433B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a type of steel and a method for manufacturing the same, and more particularly to a high-expansion steel and a method for manufacturing the same. Background Technology
[0002] In recent years, with the rapid development of the automotive industry, the market and users have put forward higher requirements for the performance of automobiles. This requires the use of superior steel plates in automobile manufacturing, such as hot-rolled plates and hot-rolled pickled plates, which have been widely used in the manufacture of chassis and wheel structure parts for passenger cars, accounting for a quarter of the steel used in automobiles.
[0003] In the actual manufacturing of passenger vehicle parts, it is often necessary to use hole expansion and partial flanging designs on steel to achieve the high strength, thinning, and lightweight requirements of the automotive industry. Research has found that the hole expansion performance of steel plates is related to the steel plate's composition, strength, and microstructure uniformity. Traditional 440MPa steel grades mainly use carbon-manganese solid solution strengthened steel and low-alloy precipitation strengthened steel, with hole expansion rates between 50% and 70%.
[0004] As automotive design places increasingly higher demands on chassis structures, the fabrication of automotive parts has become more complex. Automotive manufacturers are also continuously raising their requirements for the flanging and hole-expanding performance of steel sheets. Existing traditional carbon manganese solid solution strengthened steel and low alloy precipitation strengthened steel structural steel sheets can no longer meet the current forming requirements of automotive chassis and cantilever parts. High hole-expanding steel has become one of the important varieties of automotive steel sheets.
[0005] Currently, in response to the demand for high-expansion steel in the automotive industry, many researchers have begun to study and develop high-expansion steel sheets.
[0006] For example, Chinese patent document CN103667880A, published on March 26, 2014, entitled "A high-expansion steel plate with a tensile strength of 440MPa and its manufacturing method", discloses a high-expansion steel plate with a tensile strength of 440MPa. The product of the strength and the expansion rate of the obtained steel plate is ≥44000MPa%. However, this technical solution adds a lot of Si element in the chemical element composition design, which will lead to poor surface quality of the steel plate and fail to meet the user's high performance quality requirements.
[0007] For example, Japanese patent document with publication number JP2006063394A and publication date March 9, 2006 discloses a hot-rolled high-expansion steel with a carbon content of 0.20-0.48% and a tensile strength of ≥440MPa, but its expansion rate is only ≥70%, and it also needs to be annealed at 640℃ after hot rolling.
[0008] It is evident that the high-expansion steel plates currently developed and designed still suffer from insufficient expansion rate and poor surface quality.
[0009] Therefore, the inventors aim to provide a new high-surface-area, high-hole-expansion steel and its production method, which, based on reasonable composition design and hot rolling process, can effectively produce hot-rolled pickled products with high surface-area, high-hole-expansion performance to meet market demand. Summary of the Invention
[0010] One of the objectives of this invention is to provide a high-surface-quality, high-expansion-rate steel. This high-surface-quality, high-expansion-rate steel features high surface quality and high expansion rate, with a yield strength Rel≥305MPa, tensile strength Rm≥440MPa, elongation A≥34%, and expansion rate λ≥90%. It can meet the performance requirements of steel in applications such as automotive chassis and complex stamped parts, and has a very good prospect for promotion and application.
[0011] To achieve the above objectives, this invention proposes a high surface area and high hole expansion steel, which contains Fe and unavoidable impurities, and also contains the following chemical elements in the following mass percentages:
[0012] C: 0.02–0.08%, 0 < Si ≤ 0.1%, Mn: 0.4–1.6%, Al: 0.2–0.5%; and at least one of the following: Ti: 0.001–0.05%, Nb: 0.001–0.05%, V: 0.002–0.06%, Cr: 0.002–0.6%, Ca: 0.0005–0.0050%, REM: 0.0005–0.005%, B: 0.0002–0.0030%.
[0013] Furthermore, in the high surface area and high hole expansion steel described in this invention, the mass percentage content of each chemical element is as follows:
[0014] C: 0.02–0.08%, 0 < Si ≤ 0.1%, Mn: 0.4–1.6%, Al: 0.2–0.5%; and at least one of the following: Ti: 0.001–0.05%, Nb: 0.001–0.05%, V: 0.002–0.06%, Cr: 0.002–0.6%, Ca: 0.0005–0.0050%, REM: 0.0005–0.005%, B: 0.0002–0.0030%; the balance being Fe and other unavoidable impurities.
[0015] In the high surface area and high hole expansion steel described in this invention, the design principles of each chemical element are as follows:
[0016] C: In the high surface area and high porosity steel described in this invention, carbon (C) is sufficient to form a adequate carbide strengthening phase to ensure the steel's strength level. When the C content in the steel is too low, the steel's strength cannot meet requirements; conversely, when the C content is too high, the precipitated carbide particles are large and detrimental to the porosity expansion performance of the steel plate. Furthermore, when the carbon and manganese content in the steel is too high, coarse pearlite phases and pearlite banding structures are easily produced, which affect the steel's properties. Therefore, considering the influence of C content on steel properties, in the high surface area and high porosity steel described in this invention, the mass percentage of C is controlled between 0.02% and 0.08%.
[0017] Si: In the high surface area and high hole expansion steel described in this invention, Si can play a solid solution strengthening role in carbon manganese steel. However, the Si content in the steel should not be too high. Excessive Si content can easily cause surface defects such as red iron scale on the steel plate surface, resulting in its surface quality failing to meet the high requirements of the target user. Therefore, in the high surface area and high hole expansion steel described in this invention, the mass percentage content of Si is controlled to meet the following requirement: Si ≤ 0.1%.
[0018] Mn: In the high surface area and high porosity steel described in this invention, Mn is a solid solution strengthening element. When the Mn content in the steel is below 0.4%, the strength of the steel will be insufficient. Similarly, the Mn content should not be too high. Adding too much Mn to the steel will increase the proportion of pearlite phase and cause manganese segregation in the slab, which is one of the main causes of banded structure in steel plates. Banded structure will degrade the porosity performance of the steel plate. Therefore, the Mn content in the steel needs to be controlled below 1.6%. Based on this, in order to ensure that the steel can obtain excellent porosity performance, the mass percentage of Mn in the high surface area and high porosity steel described in this invention is controlled between 0.4% and 1.6%.
[0019] Al: In the high surface area and high porosity steel described in this invention, Al is a deoxidizing element in steel. Adding an appropriate amount of Al can effectively reduce oxide inclusions in the steel and purify the steel. Simultaneously, adding an appropriate amount of Al can also increase the Ar1 (the temperature at which austenite transforms into pearlite during cooling) and Ar3 (the starting temperature of ferrite transformation during cooling) temperatures, thereby accelerating the ferrite phase transformation and improving the formability of the steel sheet. Therefore, to maximize the beneficial effects of Al, the mass percentage of Al in the high surface area and high porosity steel described in this invention is controlled between 0.2% and 0.5%.
[0020] It should be noted that, in the high surface area and high hole expansion steel designed in this invention, in addition to the above-mentioned C, Si, Mn and Al, at least one of Ti, Nb, V, Cr, Ca, REM and B can be added to the steel according to specific needs to improve the performance of the steel.
[0021] Ti: In the high surface area and high hole expansion steel described in this invention, Ti has a strong affinity for nitrogen, oxygen, and carbon. Ti is a good deoxidizing and degassing agent and an effective element for fixing nitrogen and carbon. When Ti exists in solid solution in ferrite, it can effectively strengthen the strength of ferrite. Therefore, in this invention, an appropriate amount of Ti can be added according to actual needs, and the mass percentage of Ti can be controlled between 0.001% and 0.05%.
[0022] Niobium (Nb): In the high surface area and high porosity steel described in this invention, the strengthening effect of Nb on the steel is mainly grain refinement and dispersion strengthening. Niobium can react with carbon and nitrogen in the steel to form stable carbides and carbonitrides, and can also disperse carbides to form steel with fine grains. Therefore, in this invention, an appropriate amount of Nb can be added according to actual needs, and the mass percentage of Nb element is controlled between 0.001% and 0.05%.
[0023] V: In the high surface area and high porosity steel described in this invention, the addition of vitamin V can effectively refine the steel's microstructure and grain size, thereby increasing the grain coarsening temperature, reducing the steel's overheating sensitivity, and effectively improving its strength and toughness. Therefore, in this invention, an appropriate amount of V can be added according to actual needs, and the mass percentage of V can be controlled between 0.002% and 0.06%.
[0024] Cr: In the high surface area and high porosity steel described in this invention, chromium can form a continuous solid solution with iron, thereby improving the strength and hardness of the steel. Therefore, in this invention, an appropriate amount of Cr can be added according to actual needs, and the mass percentage of Cr can be controlled between 0.002% and 0.6%.
[0025] Ca: In the high surface area and high porosity steel described in this invention, Ca can change the morphology of sulfides in the steel and improve the plasticity and toughness of the steel plate. Therefore, the molten steel designed in this invention can be treated with calcium, and the mass percentage of Ca can be controlled between 0.0005% and 0.0050% according to actual needs.
[0026] REM: In the high surface area and high porosity steel described in this invention, modified inclusions can be added. Rare earth elements are added to the steel to form spherical rare earth sulfides or sulfur oxides, replacing elongated manganese sulfide inclusions, thus completely controlling the sulfide morphology and improving the toughness and plasticity of the steel. Therefore, in this invention, according to actual needs, an appropriate amount of REM can be added, and the mass percentage of REM element is controlled between 0.0005% and 0.005%.
[0027] B: In the high surface area and high porosity steel described in this invention, adding an appropriate amount of element B can effectively increase the hardenability of the steel and inhibit austenite recrystallization. Therefore, in this invention, an appropriate amount of element B can be added according to actual needs, and the mass percentage of element B can be controlled between 0.0002% and 0.0030%.
[0028] Furthermore, in the high surface area and high hole expansion steel described in this invention, among the unavoidable impurities, P ≤ 0.025% and S ≤ 0.003%.
[0029] In the above technical solution, P and S are both impurity elements in steel. When technical conditions permit, in order to obtain steel with better performance and higher quality, the content of impurity elements in the material should be reduced as much as possible.
[0030] P: In this invention, phosphorus (P) exacerbates component segregation in the slab during continuous casting, leading to uneven microstructure. Therefore, in the high surface area and high porosity steel described in this invention, the mass percentage of phosphorus is controlled to be P ≤ 0.025%.
[0031] S: In this invention, sulfur is an impurity element in steel. S readily forms MnS in steel, and the quantity and morphology of sulfides in the steel directly affect the porosity of the steel plate. Furthermore, the quantity and morphology of inclusion elements have a significant impact on the porosity performance of the steel plate, especially since linear sulfides can easily lead to cracking during deformation. Therefore, in the high surface area and high porosity steel described in this invention, the mass percentage of S must be strictly controlled, and the S content must be less than 0.005%, specifically controlled as S ≤ 0.003%.
[0032] Furthermore, in the high surface area and high hole expansion steel described in this invention, its microstructure is ferrite + bainite.
[0033] Furthermore, in the high surface area and high hole expansion steel of the present invention, the volume ratio of ferrite is ≥90%.
[0034] Furthermore, in the high surface area and high hole expansion steel described in this invention, its yield strength Rel≥305MPa, tensile strength Rm≥440MPa, elongation A≥34%, and hole expansion rate λ≥90%.
[0035] Accordingly, another objective of the present invention is to provide a method for manufacturing the above-mentioned high surface area and high hole expansion steel. This method is simple to produce and has a reasonable process design. The high surface area and high hole expansion steel obtained not only has a high hole expansion rate, but also has excellent surface quality, and has good application prospects.
[0036] To achieve the above objectives, the present invention provides a method for manufacturing the aforementioned high-surface-area, high-hole-expansion steel, comprising the following steps:
[0037] (1) Smelting and casting;
[0038] (2) Heating;
[0039] (3) Hot rolling: The rough rolling temperature is controlled at 990-1100℃; the finishing rolling temperature is controlled at 820-900℃; then laminar cooling and coiling are carried out.
[0040] (4) Pickling after natural cooling.
[0041] In the above technical solution of the present invention, in the smelting process of step (1), the steel composition needs to meet the chemical composition design requirements of the present invention. In addition, during smelting, LF furnace desulfurization treatment can be specifically adopted to control the sulfur content of molten steel to be less than 0.003%; after smelting is completed, the molten steel after tapping can be continuously cast to obtain slabs.
[0042] Accordingly, in some embodiments, in step (4) of the present invention, the steel coil obtained after hot rolling can be naturally cooled to below 50°C, and then the iron oxide scale on the steel plate can be removed by a pickling unit in a hot hydrochloric acid solution. Furthermore, after pickling, the steel plate obtained by pickling can be further rinsed, squeezed dry, dried, and then oiled.
[0043] Furthermore, in the manufacturing method described in this invention, in step (2), the heating temperature is controlled to be 1100-1260°C, and the furnace heating time is 160-250 min.
[0044] Furthermore, in the manufacturing method described in this invention, in step (3), the laminar cooling rate is controlled to be 30 to 200 °C / s.
[0045] Furthermore, in the manufacturing method described in this invention, in step (3), the winding temperature is controlled to be 500–660°C.
[0046] Compared with the prior art, the high surface area and high hole expansion steel and its manufacturing method described in this invention have the following advantages and beneficial effects:
[0047] This invention develops a high-surface-area, high-hole-expansion steel through reasonable chemical composition design and optimized process. The chemical composition design is superior, and the hot rolling process parameters are optimized, so that the microstructure of the steel is more than 90% ferrite and less than 10% second-phase bainite, thus ensuring the performance of the prepared steel.
[0048] The high surface area and high hole expansion steel designed in this invention has a simple composition, low cost, and a friendly hot rolling process window, making production and preparation simple.
[0049] The high-surface-quality, high-hole-expansion steel prepared using the technical solution of this invention has the characteristics of high surface quality and high hole expansion rate. Its yield strength Rel≥305MPa, tensile strength Rm≥440MPa, elongation A≥34%, and hole expansion rate λ≥90%. It can meet the requirements of steel performance for applications such as automotive chassis and complex stamped parts, and has a very good prospect for promotion and application. Attached Figure Description
[0050] Figure 1 The image shows the metallographic structure of the high-surface-area, high-hole-expansion steel of Example 1 after etching with nitric acid and alcohol, as observed under an optical microscope. Detailed Implementation
[0051] The high surface area and high hole expansion steel and its manufacturing method described in this invention will be further explained and described below with reference to the accompanying drawings and specific embodiments. However, this explanation and description do not constitute an undue limitation on the technical solution of this invention.
[0052] Examples 1-9 and Comparative Examples 1-3
[0053] The high surface area and high hole expansion steels of Examples 1-9 and the comparative steels of Comparative Examples 1-3 were all prepared using the following steps:
[0054] (1) Smelting and casting are carried out according to the chemical composition shown in Table 1 below: During smelting, desulfurization is carried out in an LF furnace to control the sulfur content of the molten steel to be less than 0.003%.
[0055] (2) Heating: The continuously cast billet obtained by continuous casting is sent to a heating furnace for heating, and the heating temperature is controlled at 1100~1260℃, and the heating time in the furnace is controlled at 160~250min.
[0056] (3) Hot rolling: The heated continuous casting billet is hot rolled, and the rough rolling temperature is controlled at 990-1100℃; the finishing rolling temperature is controlled at 820-900℃; then laminar cooling and coiling are carried out, and the laminar cooling rate is controlled at 30-200℃ / s, and the coiling temperature is controlled at 500-660℃.
[0057] (4) Pickling after natural cooling: Hot-rolled steel coils that have been naturally cooled to below 50°C are pickled in a hot hydrochloric acid solution to remove the iron oxide scale from the steel plate. After rinsing, squeezing, drying, and oiling, the pickled steel plate is treated.
[0058] In this invention, the chemical composition design and related processes of the high surface area and high hole expansion steels in Examples 1-9 all meet the design specifications of this invention. While the comparative steel plates in Comparative Examples 1-3 were also prepared using the above-described processes, their chemical composition design and / or related processes in these three embodiments do not meet the design specifications of this invention.
[0059] Table 1 lists the mass percentage of each chemical element for the high surface area and high hole expansion steels of Examples 1-9 and the comparative steels of Comparative Examples 1-3.
[0060] Table 1. (wt.%, balance is Fe and other unavoidable impurities other than P and S)
[0061]
[0062] Table 2 lists the specific process parameters for steps (1) to (4) of the above manufacturing process for the high surface area and high hole expansion steel of Examples 1-9 and the comparative steel of Comparative Examples 1-3.
[0063] Table 2.
[0064]
[0065]
[0066] It should be noted that, in this invention, after completing the above manufacturing process, samples of the high surface area and high hole expansion steel of Examples 1-9 and the comparative steel of Comparative Examples 1-3 can be taken respectively, and the surface quality of the steel plate samples of Examples 1-9 and Comparative Examples 1-3 can be observed. At the same time, the microstructure of each example and comparative example can be observed. The relevant observation and analysis results are listed in Table 3 below.
[0067] In this invention, the surface quality of the sample steel plates of each embodiment and comparative example was observed, and it was found that the surfaces of the embodiments were free of defects such as red iron oxide that could affect the coating.
[0068] Accordingly, in this invention, when observing the microstructure of the sample steel plates of each embodiment and comparative example, metallographic methods are specifically used to test the phase composition of different samples.
[0069] Table 3 lists the metallographic analysis results of the high surface area and high hole expansion steels of Examples 1-9 and the comparative steels of Comparative Examples 1-3.
[0070] Table 3.
[0071]
[0072]
[0073] As can be seen from Table 2 above, in this invention, the surface quality of the high-surface-area, high-hole-expansion steels in Examples 1-9 is relatively high, with no poor coating caused by red iron scale. Furthermore, their microstructures are all ferrite + bainite, and the volume ratio of ferrite is ≥90%, specifically between 90-98%. In contrast, in Comparative Examples 1-3, the volume ratio of ferrite in Comparative Examples 1 and 3 does not meet the requirements; the surface quality of Comparative Example 2 is poor, and its microstructure does not meet the design requirements, being only ferrite.
[0074] Accordingly, after completing the above observation and analysis of the metallographic structure, in order to further demonstrate that the high surface area and high porosity steel prepared by the present invention has excellent mechanical properties, based on the finished steel products of Examples 1-9 and Comparative Examples 1-3, the inventors again sampled these high surface area and high porosity steel products of Examples 1-9 and the comparative steel products of Comparative Examples 1-3, and further tested the performance of the sample steel plates of Examples 1-9 and Comparative Examples 1-3 to obtain the corresponding yield strength, tensile strength, elongation and porosity. The relevant test results are listed in Table 4 below.
[0075] In this invention, the specific testing methods used for the sample steel plates of Examples 1-9 and Comparative Examples 1-3 are as follows:
[0076] Tensile test: Under the conditions of GB / T 228, the strain rate during the yielding period should be controlled at 0.00025~0.0025 / s. The yield strength Rel, tensile strength Rm and elongation A of the steel plates of Examples 1-9 and Comparative Examples 1-3 were measured.
[0077] Hole expansion rate test: Take 150×150mm steel plates of each embodiment and comparative example, and use them as the initial hole diameter d[1]. Make a 10mm diameter punch and expand the punch using a conical punch with a 60° apex angle. At the same time, measure the hole diameter d[2] when the crack generated by the punch penetrates the plate thickness. Combine the above hole diameters d[1] and d[2], calculate the hole expansion rate by the following formula:
[0078] Pore expansion rate (λ) = [(d[2] - d[1]) / d[1]] × 100%
[0079] In this invention, the unit parameter of the hole expansion rate is "%". Through the above test process, the hole expansion rate λ of the sample steel plates of Examples 1-9 and Comparative Examples 1-3 can be effectively measured.
[0080] Table 4 lists the test results of the performance of the high surface area and high hole expansion steels of Examples 1-9 and the comparative steels of Comparative Examples 1-3.
[0081] Table 4.
[0082]
[0083]
[0084] As can be seen from Table 3 above, the comprehensive performance of the high surface area and high hole expansion steels of Examples 1-9 of the present invention is significantly better than that of the comparative steels of Comparative Examples 1-3.
[0085] In this invention, the high surface area and high porosity steel of Examples 1-9 has a yield strength Rel between 323-441 MPa, a tensile strength Rm between 443-526 MPa, an elongation A between 35-39%, and a porosity λ between 95-124%. It not only has good strength and plasticity, but also a high porosity and excellent surface quality.
[0086] Accordingly, by analyzing Comparative Examples 1-3 designed in this invention in conjunction with Tables 1, 2, 3, and 4, it is not difficult to find that:
[0087] In Comparative Example 1, the element content of Comparative Example 1 was not within the range required by this invention when designing its chemical composition. Its C element content was too high and its Al content was too low. The final microstructure obtained was ferrite + bainite. Although the yield strength and tensile strength of the comparative steel plate prepared by Comparative Example 1 could meet the design requirements, its porosity did not meet the requirements.
[0088] In Comparative Example 2, the element content of Comparative Example 2 was not within the range required by this invention when designing its chemical composition. Its Si content was too high, and the final microstructure obtained was ferrite. Although the yield strength, tensile strength and porosity of the comparative steel plate prepared by Comparative Example 2 could meet the design requirements, the excessive Si content in the steel could easily lead to red iron scale and fail to achieve the high surface requirements.
[0089] In Comparative Example 3, the element content of Comparative Example 3 was not within the range required by this invention when designing its chemical composition. Its C content was too high and its Al content was too low. The final microstructure obtained was ferrite + bainite. However, the elongation and porosity of the comparative steel plate prepared by Comparative Example 3 were too low and did not meet the design requirements of this invention.
[0090] By comparing Examples 1-9 with Comparative Examples 1-3, it can be seen that the technical solution designed in this invention is beneficial for obtaining steel plates with high surface area and high hole expansion performance.
[0091] Figure 1 The image shows the metallographic structure of the high-surface-area, high-hole-expansion steel of Example 1 after etching with nitric acid and alcohol, as observed under an optical microscope.
[0092] like Figure 1As shown, in this embodiment of Example 1, the microstructure of the prepared high surface area and high porosity steel is ferrite + bainite.
[0093] It should be noted that the combination of the technical features in this case is not limited to the combination methods described in the claims of this case or the combination methods described in the specific embodiments. All technical features described in this case can be freely combined or combined in any way, unless they contradict each other.
[0094] It should also be noted that the embodiments listed above are merely specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made thereto are those that can be directly derived or easily conceived by those skilled in the art from the content disclosed in the present invention, and should all fall within the protection scope of the present invention.
Claims
1. A high-surface-area, high-hole-expansion steel, characterized in that, Its mass percentage content of each chemical element is as follows: C: 0.02~0.08%, 0<Si≤0.1%, Mn: 0.4~1.6%, Al: 0.2~0.5%; and at least one of the following: Ti: 0.001~0.05%, Nb: 0.001~0.05%, V: 0.002~0.06%, Cr: 0.002~0.6%, Ca: 0.0005~0.0050%, REM: 0.0005~0.005%, B: 0.0002~0.0030%; the balance being Fe and other unavoidable impurities; The microstructure of the high surface area and high hole expansion steel is ferrite + bainite, and the volume ratio of ferrite is ≥90%. The high surface area and high hole expansion steel has a yield strength Rel≥305MPa, tensile strength Rm≥440MPa, elongation A≥34%, and hole expansion rate λ≥90%.
2. The high surface area and high hole expansion steel as described in claim 1, characterized in that, In unavoidable impurities, P ≤ 0.025% and S ≤ 0.003%.
3. The method for manufacturing high-surface-area, high-hole-expansion steel according to any one of claims 1-2, characterized in that, It includes the following steps: (1) Smelting and casting; (2) Heating; (3) Hot rolling: control the rough rolling temperature to 990-1100℃; control the finishing rolling temperature to 820-900℃; then perform laminar flow cooling and coiling; (4) Pickling after natural cooling.
4. The manufacturing method as described in claim 3, characterized in that, In step (2), the heating temperature is controlled at 1100~1260℃ and the heating time in the furnace is 160~250 min.
5. The manufacturing method as described in claim 3, characterized in that, In step (3), the laminar cooling rate is controlled to be 30~200℃ / s.
6. The manufacturing method as described in claim 3, characterized in that, In step (3), the winding temperature is controlled to be 500~660℃.
Citation Information
Patent Citations
High hole expansion steel plate with tensile strength of 440MPa and manufacturing method thereof
CN103667880A
High-carbon hot-rolled steel plate and method for manufacturing the same
JP2006063394A
Ferritomartensite hot-rolled dual phase steel with high surface quality and manufacturing method thereof
CN111363901A
High-reaming complex phase steel and manufacturing method thereof
CN112575267A