Method for growing single-crystal boron nitride on a metal substrate using a solid boron-nitrogen source
By growing single-crystal boron nitride on a metal substrate at high temperature and using a solid boron-nitrogen source for segregation deposition on the metal surface, the problems of limited catalytic activity and difficulty in controlling interlayer stacking in the traditional growth mode are solved. This enables the preparation of large-size, thickness-controllable interlayer homo-oriented stacked boron nitride, reducing preparation costs and energy consumption.
Patent Information
- Application Number
- CN202310015768.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-05
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-01-05
AI Technical Summary
Existing technologies make it difficult to prepare large-sized, thick-layer boron nitride crystals with controllable thickness and interlayer homo-oriented stacking. Traditional growth methods suffer from limitations in catalytic activity and difficulties in controlling interlayer stacking.
A method for growing single-crystal boron nitride on a metal substrate at high temperature using a solid boron-nitrogen source involves forming a stack of solid boron-nitrogen source and metal substrate, growing it at high temperature, and segregating and depositing the solid boron-nitrogen source on the metal surface to achieve interlayer co-orientation stacking.
It has enabled the growth of large-area, thickness-controllable single-crystal boron nitride, reducing substrate cost and energy consumption, and providing a material basis for wide applications.
Smart Images

Figure CN117512781B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of two-dimensional material growth technology, and in particular relates to a method for growing single-crystal boron nitride on a metal substrate using a solid boron-nitrogen source. Background Technology
[0002] In recent years, thick-layer hexagonal boron nitride has played a crucial role in emerging optical applications such as mid-infrared phonon polarization, room-temperature single-photon emission, and deep-ultraviolet emission and detection. Meanwhile, the consistent orientation of the interlayer stacking not only preserves the spatial inversion asymmetry inherent in monolayer boron nitride, enabling coherent growth of second-order nonlinear signals with increasing layer count, but also introduces new out-of-plane polarization, achieving atomically thin, non-volatile ferroelectric memory functionality. Therefore, fabricating thick-layer boron nitride with identically oriented interlayer stacking has become key to its application in novel fields such as miniaturized laser generation, ferroelectric storage, and quantum light sources.
[0003] Currently, there are two main methods for preparing hexagonal boron nitride: one is a top-down growth mode based on chemical vapor deposition (CVD), which utilizes the rich surface structure of the substrate to control the orientation of boron nitride; the other is a bottom-up growth mode based on the dissolution and precipitation of boron-nitrogen sources in liquid metal solvents, which can achieve the preparation of thick-layer boron nitride. However, the top-down growth mode, due to the limitation of substrate catalytic activity, can often only prepare boron nitride films with a limited number of layers; while in the bottom-up growth mode, the interlayer stacking of boron nitride relies solely on the control of its weak van der Waals forces, often resulting in thick crystals with the lowest energy and antiparallel interlayer stacking. Therefore, simultaneously leveraging the advantages of both growth modes to achieve the preparation of large-size, thickness-controllable, and co-oriented thick-layer boron nitride crystals is a technical challenge that urgently needs to be solved. Summary of the Invention
[0004] This disclosure provides at least one embodiment of a method for growing single-crystal boron nitride on a metal substrate, the method comprising the following steps:
[0005] (i) A solid boron-nitrogen source is placed under a metal substrate to form a laminate;
[0006] (ii) The laminate is heated to a predetermined temperature and then kept at the predetermined temperature for 0.1-100h; wherein the predetermined temperature range is 1000-1400℃.
[0007] For example, the solid boron-nitrogen source includes one or more raw materials selected from hot-pressed boron nitride paper, boron nitride powder, boron powder, iron boride powder, iron nitride powder, chromium boride powder, and chromium nitride powder.
[0008] For example, the metal substrate is a metal foil made of iron, nickel, iron-nickel alloy, iron-chromium alloy, or nickel-chromium alloy.
[0009] For example, the metal substrate is 1-200 micrometers thick, preferably 10-120 micrometers thick.
[0010] In one embodiment, the heating of the laminate to a predetermined temperature is carried out at a constant rate of 5-30°C / min.
[0011] In one embodiment, heating the laminate to a predetermined temperature is performed in an atmosphere of one or more gases selected from nitrogen, argon, and hydrogen. For example, heating the laminate to the predetermined temperature is performed at atmospheric pressure in an atmosphere of nitrogen and hydrogen. Preferably, the atmosphere optionally further includes argon, with argon and hydrogen flow rates of 0-1000 sccm and 10-100 sccm, respectively.
[0012] For example, the flow rate of the nitrogen gas is 100-1000 sccm.
[0013] In one embodiment, heating the laminate to a predetermined temperature is performed by placing the laminate on a high-temperature resistant plate and then placing it together in a tube furnace. For example, the high-temperature resistant plate may be a quartz plate, a corundum plate, or a boron nitride plate.
[0014] In one implementation, after the growth is carried out under heat, the heating power is turned off, the gas atmosphere is kept constant, and the laminate is allowed to cool naturally to room temperature.
[0015] In one embodiment, a pretreatment step of the metal substrate is included before step (i), wherein the pretreatment refers to annealing industrial metal foil in a reducing gas at 1200-1550°C for 1-20 hours.
[0016] In one embodiment, the metal substrate is a single-crystal metal substrate or a polycrystalline metal substrate. For example, the metal substrate is a single-crystal metal substrate of nickel or an iron-nickel alloy. Preferably, the metal substrate is a single-crystal substrate with a maximum crystal size of 5 cm. 2 Single-crystal metal substrate.
[0017] In one implementation, the grown single-crystal boron nitride is stacked in the same orientation between layers.
[0018] For example, the thickness of the grown single-crystal boron nitride is 0.01-10 μm.
[0019] In one implementation, the grown single-crystal boron nitride can reach a maximum size of 5 cm. 2 .
[0020] This disclosure primarily utilizes the continuous decomposition of a solid boron-nitrogen source at high temperatures, dissolving it in a metal foil and diffusing within it, ultimately segregating from the metal surface to deposit a thick layer of single-crystal boron nitride. This disclosure provides an effective means of controlling the preparation of large-area, thickness-controllable boron nitride crystals and proposes a novel approach to achieving co-oriented stacking of boron nitride layers based on a solid substrate, laying the material foundation for various functional applications of boron nitride crystals.
[0021] This disclosure has one or more of the following advantages:
[0022] 1. This disclosure can use commercially available polycrystalline metal foil, which does not require complex surface treatment. The corresponding large-size single crystal substrate can be prepared by high-temperature annealing alone, which greatly reduces the substrate cost.
[0023] 2. Compared with the extreme environment (such as ultra-high temperature and pressure) required for the preparation of traditional boron nitride crystals, the crystal preparation temperature and pressure used in this disclosure can be achieved in a conventional tube furnace, which reduces energy consumption and preparation cost;
[0024] 3. The solid-state source transport growth mode proposed in this disclosure can ensure the continuous growth of boron nitride crystals, and the prepared single-crystal boron nitride has a large size and a large number of layers;
[0025] 4. By designing the surface structure of a solid substrate and controlling the consistent orientation of each layer during growth, thick-layer boron nitride is prepared with a parallel stacking interlayer configuration, which has broad application prospects. Attached Figure Description
[0026] To more clearly illustrate the technical solutions of the embodiments of this disclosure, the accompanying drawings of the embodiments will be briefly described below. Obviously, the drawings described below only relate to some embodiments of this disclosure and are not intended to limit the invention.
[0027] Figure 1 This is a schematic diagram of the process of growing single-crystal boron nitride according to an embodiment of the present disclosure.
[0028] Figure 2 This is a physical image (left) and a scanning electron microscope photograph (right) of a thick-layer single-crystal boron nitride prepared according to an embodiment of this disclosure.
[0029] Figure 3 This is an atomic-resolution structural characterization of interlayer isooriented stacked boron nitride prepared according to an embodiment of this disclosure. Left: Planar high-resolution transmission electron microscope image; Right: Cross-sectional atomic-resolution scanning transmission electron microscope image.
[0030] Figure 4 The crystal quality characterization of a single-crystal boron nitride prepared according to an embodiment of this disclosure includes a Raman spectrum (left), a UV-Vis absorption spectrum (middle), and an X-ray diffraction spectrum (right). Detailed Implementation
[0031] To make the objectives, technical solutions, and advantages of the embodiments of this disclosure clearer, the technical solutions of the embodiments of this disclosure will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this disclosure. All other embodiments obtained by those skilled in the art based on the described embodiments of this disclosure without creative effort are within the scope of protection of this invention.
[0032] This invention may be implemented in other specific forms without departing from its essential attributes. It should be understood that, without conflict, any and all embodiments of this invention can be combined with technical features of any or more other embodiments to obtain further embodiments. This invention includes such combinations to obtain further embodiments.
[0033] All publications and patents mentioned in this disclosure are incorporated herein by reference in their entirety. In the event of any conflict between the use or terminology used in any publications and patents incorporated by reference and the use or terminology used in this disclosure, the use and terminology of this disclosure shall prevail.
[0034] The chapter titles used in this article are for organizational purposes only and should not be construed as limiting the subject matter.
[0035] Unless otherwise specified, all technical and scientific terms used herein have their usual meaning in the field to which the claimed subject matter pertains. Where multiple definitions exist for a term, the definition herein shall prevail.
[0036] As used herein, the words “comprising,” “containing,” or “including” mean that the element preceding the word encompasses the elements listed following the word and their equivalents, without excluding elements not described. The terms “containing” or “comprising (including)” as used herein can be open-ended, semi-closed, or closed-ended. In other words, the terms also include “consistently composed of” or “composed of”.
[0037] It should be understood that the singular form used in this disclosure (such as "a") may include plural references unless otherwise specified.
[0038] The reagents and raw materials used in this disclosure are commercially available or can be prepared by conventional methods.
[0039] Unless otherwise stated, when any type of range (e.g., thickness) is disclosed or claimed, the intention to separately disclose or claim each possible numerical value that range may reasonably encompass, including any sub-ranges included therein. For example, numerical ranges of thickness herein, such as 1 to 120 micrometers, indicate thicknesses within that range, where 1-120 micrometers should be understood to include 1, 2, 3, 4, 5, 6, 7, 8, 9, 10...120 micrometers, as well as ranges of 1-5 and 1-10. Except as indicated in the working examples or otherwise, all figures set forth in the specification and claims expressing the amount of material, reaction conditions, incubation growth time, quantitative properties of the material, etc., should be understood to be modified by the term "about" in all cases. It should also be understood that any numerical range listed in this application is intended to include all sub-ranges within that range and any combination of the endpoints of that range or sub-ranges.
[0040] like Figure 1 As shown, this disclosure mainly utilizes the continuous decomposition of a solid boron-nitrogen source at high temperature, dissolving it in a metal foil and diffusing within it, ultimately segregating from the metal surface to deposit a thick layer of single-crystal boron nitride. This disclosure provides an effective means of controlling the preparation of large-area, thickness-controllable boron nitride crystals, and proposes a new approach to achieve co-orientation stacking of boron nitride layers based on a solid substrate, laying the material foundation for various functional applications of boron nitride crystals.
[0041] This disclosure provides a method for growing single-crystal boron nitride on a metal substrate, the method comprising the following steps:
[0042] (i) A solid boron-nitrogen source is placed under a metal substrate to form a laminate;
[0043] (ii) The laminate is heated to a predetermined temperature and then kept at the predetermined temperature for 0.1-100h; wherein the predetermined temperature range is 1000-1400℃.
[0044] The laminate is heated to a predetermined temperature, which should be lower than the melting temperature of the metal substrate, for example, 100-400°C lower than the melting temperature of the metal substrate. For example, the predetermined temperature is 1000, 1020, 1050, 1100, 1150, 1200, 1250, 1300, 1350, or 1400°C. In one embodiment, the laminate is heated to the predetermined temperature at a constant rate of 5-30°C / min, for example, at 5°C / min, 10°C / min, 15°C / min, 20°C / min, 25°C / min, or 30°C / min.
[0045] In one embodiment, heating the laminate to a predetermined temperature is performed in an atmosphere of one or more gases selected from nitrogen, argon, and hydrogen.
[0046] For example, heating the laminate to a predetermined temperature is performed at atmospheric pressure in an atmosphere of nitrogen and hydrogen. In one embodiment, the nitrogen flow rate is 100-1000 sccm, and the hydrogen flow rate is 10-100 sccm. In a preferred embodiment, the atmosphere optionally further includes argon, with argon and hydrogen flow rates of 0-1000 sccm and 10-100 sccm, respectively.
[0047] In one embodiment, heating the laminate to a predetermined temperature is performed by placing the laminate on a high-temperature resistant plate and then placing it together in a tube furnace. For example, the high-temperature resistant plate may be a quartz plate, a corundum plate, or a boron nitride plate.
[0048] In one embodiment, a pretreatment step is included before step (i) of the metal substrate, wherein the pretreatment refers to annealing an industrial metal foil at 1200-1550°C for 1-20 hours in a reducing gas. The reducing gas is, for example, a mixture of Ar and H2, with a volume ratio of Ar:H2 = 0.5:1 to 200:1, and flow rates of Ar and H2 of 100-1000 sccm and 5-200 sccm, respectively.
[0049] Incubate and grow at a predetermined temperature for 0.1-100 hours, for example, 0.1, 0.2, 0.3, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 20, 30, 40, 50, 60, 70, 80, 90, or 100 hours.
[0050] In one implementation, after the growth is carried out under heat, the heating power is turned off, the gas atmosphere is kept constant, and the laminate is allowed to cool naturally to room temperature.
[0051] A solid boron-nitrogen source refers to a raw material in solid form that provides boron and / or nitrogen for the growth of single-crystal boron nitride. For example, a solid boron-nitrogen source is hot-pressed boron nitride paper or boron nitride powder, which can simultaneously provide boron and nitrogen for the growth of single-crystal boron nitride. For example, a solid boron-nitrogen source is boron powder, iron boride powder, or chromium boride powder, which can provide boron for the growth of single-crystal boron nitride, while nitrogen can be obtained from a nitrogen atmosphere. For example, a solid boron-nitrogen source is a mixed powder of iron boride and iron nitride or a mixed powder of chromium boride and chromium nitride, which can simultaneously provide boron and nitrogen for the growth of single-crystal boron nitride. The purity of the solid boron-nitrogen source in this application is typically 99.0% or higher. In one embodiment, the purity of the solid boron-nitrogen source is 99.5% or higher. In a preferred embodiment, the purity of the solid boron-nitrogen source is 99.9% or higher.
[0052] In one embodiment, the solid boron-nitrogen source comprises one or more raw materials selected from hot-pressed boron nitride paper, boron nitride powder, boron powder, iron boride powder, iron nitride powder, chromium boride powder, and chromium nitride powder. For example, the solid boron-nitrogen source is a mixture of hot-pressed boron nitride paper, boron nitride powder, boron powder, iron boride and iron nitride powder, or a mixture of chromium boride and chromium nitride powder. The purity of the metal substrate in this application is typically 98.0% or higher. In one embodiment, the purity of the metal substrate is 99.0% or higher. In a preferred embodiment, the purity of the metal substrate is 99.5% or higher. In a more preferred embodiment, the purity of the metal substrate is 99.9% or higher. In an even more preferred embodiment, the purity of the metal substrate is 99.99% or higher.
[0053] In one embodiment, the metal substrate is a metal foil made of iron, nickel, iron-nickel alloy, iron-chromium alloy, or nickel-chromium alloy.
[0054] In one embodiment, the metal substrate is a single-crystal metal substrate or a polycrystalline metal substrate. The metal substrate may be, for example, a highly crystalline iron foil, a single-crystal iron-nickel alloy foil, a single-crystal nickel foil, a highly crystalline nickel-chromium alloy foil, or a highly crystalline iron-chromium alloy foil.
[0055] In a preferred embodiment, the metal substrate is a single-crystal metal substrate of nickel or an iron-nickel alloy. In a more preferred embodiment, the metal substrate is a single-crystal substrate with a maximum crystal size of 5 cm. 2 Single-crystal metal substrate.
[0056] In one embodiment, the metal substrate is 1-200 micrometers thick, preferably 10-120 micrometers thick, for example, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 6 3, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100, 101, 102, 103, 104, 105, 106, 107, 108, 109, 110, 111, 112, 123, 114, 115, 116, 117, 118, 119, and 120 micrometers thick.
[0057] The metal substrate can be commercially available or fabricated using conventional techniques.
[0058] In one embodiment, providing a metal substrate includes the following steps:
[0059] (1) Place industrial polycrystalline metal foil on a high-temperature resistant substrate such as a quartz plate, corundum plate or boron nitride plate, and place it in a tube furnace;
[0060] (2) Inert protective gas is introduced into the tube furnace and the temperature is raised to 1200-1550℃ at a constant rate of 5-30℃ / min;
[0061] (3) Anneal the metal foil at 1200-1550℃ for 1-20 hours;
[0062] (4) After the annealing time is over, maintain the gas flow rate in the tubular furnace and allow it to cool naturally to room temperature.
[0063] For example, the industrial polycrystalline metal foil mentioned in step (1) includes iron, nickel, iron-nickel alloy, iron-chromium alloy, or nickel-chromium alloy.
[0064] For example, the flow rates of argon and hydrogen in the inert protective gas in step (2) are 100-1000 sccm and 10-100 sccm, respectively.
[0065] For example, the preparation and characterization of single-crystal nickel foil can be found in Nature, 2020, Vol. 581, pp. 406-410, “Seeded growth of large single-crystal copper foils with high-index facets”. For instance, the nickel foil (100 micrometers thick, 99.994%, Alfa Aesar) was first oxidized in air at 150-650°C for 1-4 hours, and then annealed in a reducing atmosphere at 1300°C for 3-6 hours. After thermal annealing, a foil with a size of approximately 5 cm was obtained. 2 Single-crystal nickel foil. Several high-index single-crystal nickel foils can be produced by repeating a typical annealing process. Single-crystal nickel foils can be characterized by X-ray diffraction (XRD) and electron backscatter diffraction (EBSD).
[0066] For example, single-crystal nickel foil can be provided through the following steps:
[0067] S11, place polycrystalline nickel foil on a high-temperature resistant substrate and pre-oxidize it at 150-650℃ for 1-5 hours;
[0068] S12, introduce inert protective gas, and then heat to 1000-1350℃ within 60-120 minutes;
[0069] S13, annealing process of nickel foil at 1000-1350℃ for 1-20h;
[0070] S14, after the annealing time is over, the atmosphere conditions remain unchanged and the mixture is cooled to room temperature to obtain a single crystal nickel foil.
[0071] In one embodiment, steps S11-S14 are carried out in a tubular furnace.
[0072] The pre-oxidation in step S11 can be carried out in an oxygen or air atmosphere.
[0073] In a preferred embodiment, the inert protective gas in step S12 is a mixture of nitrogen and H2, or a mixture of Ar and H2, or a mixture of nitrogen, Ar, and H2. In a more preferred embodiment, the inert protective gas in step S12 is a mixture of Ar and H2. In an even more preferred embodiment, the inert protective gas in step S12 is a mixture of Ar and H2, with an Ar:H2 volume ratio of 0.5:1 to 200:1. In an even more preferred embodiment, the flow rates of Ar and H2 in step S12 are 100-1000 sccm and 5-200 sccm, respectively.
[0074] In step S11, the high-temperature resistant substrate can be a quartz or corundum substrate, and the tube furnace in steps S11-S14 can be a quartz furnace or a corundum furnace. For example, the selection of the high-temperature resistant substrate and the tube furnace in step S11 is related to the annealing temperature. Quartz material is selected when the annealing temperature is 1000-1150℃, and corundum material is selected when the annealing temperature is 1150-1350℃.
[0075] In one embodiment, the grown single-crystal boron nitride is stacked in the same orientation between layers. For example, the thickness of the grown single-crystal boron nitride is 0.01-10 μm.
[0076] In one implementation, the grown single-crystal boron nitride can reach a maximum size of 5 cm. 2 .
[0077] Interlayer co-orientation stacking refers to the parallel arrangement of two adjacent boron nitride layers. Corresponding thick boron nitride layers include Bernal (AB) stacking, Rhombohedral (ABC) stacking, and a combination of both. In contrast, in traditional boron nitride, adjacent layers are arranged antiparallel or rotated 180 degrees, i.e., AA' stacking.
[0078]
[0079] Optical properties of unidirectional stacked boron nitride
[0080] Single-layer hexagonal boron nitride (BN) can generate optical second harmonic signals due to the breaking of its central inversion symmetry; for example, light incident at 800 nm can produce light at 400 nm. However, BN stacked with co-oriented layers retains this inversion asymmetry, and the generated second harmonic signal exhibits a square-dependent relationship with increasing layer number. For instance, for the same 40 nm thick BN, the second harmonic signal generated by co-oriented stacking is five orders of magnitude stronger than that from anti-co-oriented stacking. Therefore, thick single-crystal BN films with co-oriented stacking can achieve highly efficient optical frequency conversion, providing a solid material foundation for the development of modern miniaturized and micro-miniaturized optical lasers, quantum optical chips, and other applications.
[0081] The metal substrate beneath the single-crystal boron nitride disclosed herein can be removed using conventional methods. For example, a fresh ferric chloride solution is prepared, the prepared sample is placed in the solution, and left to stand for 1 hour to 5 days. The ferric chloride reacts with the metal substrate, thereby etching away the metal substrate. The resulting sample is then placed in deionized water and rinsed several times to finally obtain the transferred single-crystal boron nitride sample.
[0082] The single-crystal boron nitride disclosed herein can also be used to obtain single-crystal boron nitride films via mechanical exfoliation: specifically, adhesive tape is adhered to the prepared single-crystal boron nitride, then peeled off, and attached to any substrate. After appropriate heating, the adhesive tape is then peeled off, revealing the exfoliated single-crystal boron nitride sample on the substrate. Because the prepared single-crystal boron nitride is of very high quality, the peeled sample is extremely pure and consistent with intrinsic single-crystal boron nitride.
[0083] The method disclosed herein has one or more of the following advantages:
[0084] 1. This disclosure uses commercially available polycrystalline metal foil, which does not require complex surface treatment. The corresponding large-size single-crystal substrate can be prepared simply by high-temperature annealing, which greatly reduces the substrate cost.
[0085] 2. Compared with the extreme environment (such as ultra-high temperature and pressure) required for the preparation of traditional boron nitride crystals, the crystal preparation temperature and pressure used in this disclosure can be achieved in a conventional tube furnace, which reduces energy consumption and preparation cost;
[0086] 3. The solid-state source transport growth mode proposed in this disclosure can ensure the continuous growth of boron nitride crystals, and the prepared single-crystal boron nitride has a large size and a large number of layers;
[0087] 4. By designing the surface structure of a solid substrate and controlling the consistent orientation of each layer during growth, thick-layer boron nitride is prepared with a parallel stacking interlayer configuration, which has broad application prospects.
[0088] The present invention will be further described in detail below with reference to specific embodiments, but the method of the present invention is not limited to the following embodiments. Unless otherwise specified, the steps in the following embodiments are conventional operations; unless otherwise specified, the raw materials can be obtained from publicly available commercial sources.
[0089] Example 1:
[0090] A method for preparing single-crystal boron nitride is provided, the method comprising the following steps:
[0091] (i) Select a highly crystalline iron foil (100 micrometers thick, 99.994%, Alfa Aesar) as a substrate, place it on hot-pressed boron nitride paper, and place it in a tube furnace;
[0092] (ii) Nitrogen (1000 sccm) and reducing gas (argon: 0 sccm; hydrogen: 100 sccm) are introduced into a tube furnace and the temperature is raised to 1250℃ at a constant rate of 20℃ / min.
[0093] (iii) Thick-layer boron nitride was grown at 1250℃ for 100 h;
[0094] (iv) After the annealing time is over, maintain the gas flow rate in the tubular furnace and allow it to cool naturally to room temperature.
[0095] The obtained single-crystal boron nitride is a thick-layer single-crystal boron nitride with interlayer homo-oriented stacking, and the largest single crystal area is 2 cm². 2 The thickness is 10μm.
[0096] Figure 2 The images show a physical photograph (left) and a scanning electron microscope image (right) of the thick-layer single-crystal boron nitride prepared in Example 1.
[0097] Figure 3 This is an atomic-resolution structural characterization of the interlayer isooriented stacked boron nitride prepared in Example 1. Left: Planar high-resolution transmission electron microscope image; Right: Cross-sectional atomic-resolution scanning transmission electron microscope image.
[0098] Figure 4 The crystal quality characterization of the single-crystal boron nitride prepared in Example 1 includes Raman spectrum (left), ultraviolet-visible absorption spectrum (middle), and X-ray diffraction spectrum (right).
[0099] Characterization results show that the boron nitride we prepared has very few defects, an ultra-large optical band gap, and a consistent out-of-plane orientation.
[0100] Example 2:
[0101] A method for preparing single-crystal boron nitride is provided, the method comprising the following steps:
[0102] (i) Select a highly crystalline iron foil (100 micrometers thick, 99.994%, Alfa Aesar) as a substrate, place it on boron nitride powder, and place it in a tube furnace;
[0103] (ii) Nitrogen (400 sccm) and reducing gas (argon: 500 sccm; hydrogen: 70 sccm) are introduced into a tube furnace and the temperature is raised to 1200℃ at a constant rate of 30℃ / min.
[0104] (iii) Thick-layer boron nitride was grown at 1200℃ for 70 hours;
[0105] (iv) After the annealing time is over, maintain the gas flow rate in the tubular furnace and allow it to cool naturally to room temperature.
[0106] The obtained single-crystal boron nitride is a thick-layer single-crystal boron nitride with interlayer homo-oriented stacking, and the largest single crystal area is 1 cm². 2 The thickness is 5 μm, and the characterization results are similar to those of Example 1, and are not shown.
[0107] Example 3:
[0108] A method for preparing single-crystal boron nitride is provided, the method comprising the following steps:
[0109] (i) Select single crystal iron-nickel alloy foil (4J42, Xi'an Steel Research Institute) as the substrate, place it on boron powder, and put it in a tube furnace;
[0110] (ii) Nitrogen (600 sccm) and reducing gas (argon: 300 sccm; hydrogen: 30 sccm) are introduced into a tube furnace and the temperature is raised to 1000℃ at a constant rate of 20℃ / min.
[0111] (iii) Thick-layer boron nitride was grown at 1000℃ for 30 hours;
[0112] (iv) After the annealing time is over, maintain the gas flow rate in the tubular furnace and allow it to cool naturally to room temperature.
[0113] The obtained single-crystal boron nitride is a thick-layer single-crystal boron nitride with interlayer homo-oriented stacking, and the largest single crystal area is 5 cm². 2 The thickness is 1 μm, and the characterization results are similar to those of Example 1, and are not shown.
[0114] Example 4:
[0115] A method for preparing single-crystal boron nitride is provided, the method comprising the following steps:
[0116] (i) Select single crystal iron-nickel alloy foil (4J42, Xi'an Steel Research Institute) as the substrate, place it on a mixture of iron boride and iron nitride powder, and place it in a tube furnace;
[0117] (ii) Nitrogen (200 sccm) and reducing gas (argon: 800 sccm; hydrogen: 50 sccm) are introduced into a tube furnace, and the temperature is raised to 1050℃ at a constant rate of 5℃ / min.
[0118] (iii) Thick-layer boron nitride was grown at 1050℃ for 0.1 h;
[0119] (iv) After the annealing time is over, maintain the gas flow rate in the tubular furnace and allow it to cool naturally to room temperature.
[0120] The obtained single-crystal boron nitride is a thick-layer single-crystal boron nitride with interlayer homo-oriented stacking, and the largest single crystal area is 5 cm². 2 The thickness is 0.01 μm, and the characterization results are similar to those of Example 1, and are not shown.
[0121] Example 5:
[0122] A method for preparing single-crystal boron nitride is provided, the method comprising the following steps:
[0123] (i) Select a single crystal nickel foil (100 micrometers thick, 99.994%, Alfa Aesar) as a substrate, place it on a mixed powder of chromium boride and chromium nitride, and place it in a tube furnace;
[0124] (ii) Nitrogen (100 sccm) and reducing gas (argon: 1000 sccm; hydrogen: 10 sccm) are introduced into a tube furnace and the temperature is raised to 1350℃ at a constant rate of 10℃ / min.
[0125] (iii) Thick-layer boron nitride was grown at 1350℃ for 5 hours;
[0126] (iv) After the annealing time is over, maintain the gas flow rate in the tubular furnace and allow it to cool naturally to room temperature.
[0127] The obtained single-crystal boron nitride is a thick-layer single-crystal boron nitride with interlayer homo-oriented stacking, and the largest single crystal area is 5 cm². 2 The thickness is 0.2 μm, and the characterization results are similar to those of Example 1, and are not shown.
[0128] Example 6:
[0129] A method for preparing single-crystal boron nitride is provided, the method comprising the following steps:
[0130] (i) Select a highly crystalline nickel-chromium alloy foil (50 micrometers thick, 000125, PrMat) as a substrate, place it on boron powder, and put it in a tube furnace.
[0131] (ii) Nitrogen (500 sccm) and reducing gas (argon: 500 sccm; hydrogen: 50 sccm) are introduced into a tube furnace and the temperature is raised to 1300℃ at a constant rate of 10℃ / min.
[0132] (iii) Thick-layer boron nitride was grown at 1300℃ for 40 hours;
[0133] (iv) After the annealing time is over, maintain the gas flow rate in the tubular furnace and allow it to cool naturally to room temperature.
[0134] The obtained single-crystal boron nitride is a thick-layer single-crystal boron nitride with interlayer homo-oriented stacking, and the largest single crystal area is 3 cm². 2 The thickness is 4 μm, and the characterization results are similar to those of Example 1, and are not shown.
[0135] Example 7:
[0136] A method for preparing single-crystal boron nitride is provided, the method comprising the following steps:
[0137] (i) Select a highly crystalline iron-chromium alloy foil (100 micrometers thick, 000161, PrMat) as a substrate, place it on hot-pressed boron nitride paper, and place it in a tube furnace.
[0138] (ii) Nitrogen (800 sccm) and reducing gas (argon: 200 sccm; hydrogen: 100 sccm) are introduced into a tube furnace and the temperature is raised to 1400℃ at a constant rate of 5℃ / min.
[0139] (iii) Thick-layer boron nitride was grown at 1400℃ for 20 hours;
[0140] (iv) After the annealing time is over, maintain the gas flow rate in the tubular furnace and allow it to cool naturally to room temperature.
[0141] The obtained single-crystal boron nitride is a thick-layer single-crystal boron nitride with interlayer homo-oriented stacking, and the largest single crystal area is 2 cm². 2 The thickness is 2 μm, and the characterization results are similar to those of Example 1, and are not shown.
[0142] Although specific embodiments of the present invention have been described in detail, those skilled in the art will understand that various modifications and substitutions can be made to those details based on the above-disclosed teachings, and all such changes are within the scope of protection of the present invention. The scope of protection of the present invention is determined by the appended claims and their equivalents.
Claims
1. A method for growing single crystal boron nitride on a metal substrate, the method comprising the steps of: (i) placing a solid boron-nitrogen source below a metal substrate to form a stack; (ii) raising the temperature of the layered body to a predetermined temperature, and then growing at the predetermined temperature for 0.1 to 100 hours; wherein the predetermined temperature range is 1000-1400 °C, wherein the metal substrate is a metal foil consisting of iron, nickel, iron-nickel alloy, iron-chromium alloy, or nickel-chromium alloy; wherein during the isothermal growth, the solid boron-nitrogen source continuously decomposes, dissolves into the metal substrate and diffuses therein, and precipitates on the surface of the metal substrate away from the solid boron-nitrogen source to grow single crystal boron nitride, wherein the grown single crystal boron nitride is interlaminar homo-epitaxial.
2. The method of claim 1, wherein, the solid boron-nitrogen source is selected from one or more of hot-pressed boron nitride paper, boron nitride powder, boron powder, ferroboron powder, mixed powder of ferroboron and ferronitride, chromoboron powder, and mixed powder of chromoboron and chromonitride.
3. The method of claim 1, wherein, the metal substrate is 1-200 microns thick.
4. The method of claim 3, wherein, the metal substrate is 10-120 microns thick.
5. The method of claim 1, wherein the heating the stack to the predetermined temperature is performed at a constant rate of 5-30 °C / min.
6. The method of claim 1, wherein the heating the stack to the predetermined temperature is performed in an atmosphere of one or more gases selected from nitrogen, argon, and hydrogen.
7. The method of claim 6, wherein the heating the stack to the predetermined temperature is performed in an atmosphere of nitrogen and hydrogen at normal pressure.
8. The method of claim 7, wherein, the atmosphere optionally further comprises argon at a flow rate of 0-1000 seem, and hydrogen at a flow rate of 10-100 seem.
9. The method of claim 7, wherein, the nitrogen is at a flow rate of 100-1000 seem.
10. The method of claim 1, wherein the heating the stack to the predetermined temperature is performed by placing the stack on a high-temperature resistant plate and together in a tube furnace.
11. The method of claim 1, wherein after the isothermal growth, the heating power is turned off, the gas atmosphere is maintained, and the stack is naturally cooled to room temperature.
12. The method of claim 1, wherein prior to step (i), the method further comprises a step of pretreating the metal substrate, wherein the pretreatment is annealing the industrial metal foil in a reducing gas at 1200-1550 °C for 1-20 h.
13. The method of claim 1, wherein the metal substrate is a single-crystal metal substrate or a polycrystalline metal substrate.
14. The method of claim 13, wherein the metal substrate is a single-crystal metal substrate of nickel or iron-nickel alloy.
15. The method of claim 14, wherein the metal substrate is a single crystal metal substrate having a maximum single crystal dimension of 5 cm 2 .
16. The method of claim 10, wherein the high-temperature resistant plate comprises a quartz plate, a corundum plate, or a boron nitride plate.
17. The method of any one of claims 1-16, wherein the grown single crystal boron nitride has a thickness of 0.01-10 μm.
18. The method of any one of claims 1-16, wherein the grown single-crystal boron nitride is up to 5 cm in size. 2 .
Citation Information
Patent Citations
Method for improving quality of large hexagonal phase boron nitride single crystal
CN111334850A