Microlens fabrication method

By fabricating metal templates on OLED devices, the use of developing solutions or stripping solutions is avoided, the corrosion problem of microlens fabrication on OLED devices is solved, and the process is simplified and the lifespan is extended.

CN117518308BActive Publication Date: 2026-11-20ZHEJIANG HONGXI TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311228388.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-21
Publication Date
2026-11-20
Estimated Expiration
2043-09-21

AI Technical Summary

Technical Problem

In existing microlens fabrication methods, prolonged immersion in developing or stripping solutions can corrode OLED devices and affect their lifespan.

Method used

A metal template is fabricated using patterning and electroplating processes. Microlenses are then formed on the substrate structure using the metal template, avoiding the use of developing or stripping solutions. The process includes fabricating an insulating layer on a metal substrate, patterning to form microstructures, electroplating to form a metal template, injecting photoresist and heating to soften it to form hemispherical microlenses, and finally covering it with a transparent filler layer.

Benefits of technology

It simplifies the microlens manufacturing process, enables mass production of microlenses, avoids corrosion of OLED devices, and extends their lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117518308B_ABST
    Figure CN117518308B_ABST
Patent Text Reader

Abstract

The micro-lens manufacturing method disclosed by the present disclosure belongs to the field of optical technology. The micro-lens manufacturing method comprises the following steps: manufacturing an insulating layer on a metal substrate; performing a patterning process on the insulating layer to obtain a first micro-structure, wherein the first micro-structure comprises a plurality of first units arranged in an array; performing electroplating by using the metal substrate as a cathode to form a metal template on the micro-structure, wherein the metal template has a plurality of micro-grooves arranged in an array; injecting photoresist into the micro-grooves of the metal template and covering a substrate structure; removing the metal template to form a second micro-structure on the cover plate, wherein the second micro-structure comprises a plurality of second units arranged in an array; heating the second micro-structure to soften the surface of each second unit of the second micro-structure into a spherical surface; covering the second micro-structure with a transparent filling layer to obtain a micro-lens, wherein the transmittance of the transparent filling layer is greater than that of the second micro-structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of optical technology, and in particular to a method for fabricating a microlens. Background Technology

[0002] Microlenses at the micro-nano scale are commonly used in organic light-emitting diode (OLED) displays, primarily for focusing, imaging, and beam conversion.

[0003] A method for fabricating microlenses is provided in the related technology. The method includes: spin-coating photoresist on an OLED device, and then developing and exposing the photoresist to form a microlens structure.

[0004] Whether the developing solution is strongly alkaline or weakly alkaline, prolonged immersion in it can corrode the organic light-emitting materials in OLED devices, directly and fatally impacting their lifespan. Summary of the Invention

[0005] This disclosure provides a method for fabricating microlenses, which avoids corrosion caused by immersion in developing or stripping solutions, thus preventing the microlens fabrication from having a fatal impact on the lifespan of OLED devices. The technical solution is as follows:

[0006] This disclosure provides a method for fabricating a microlens, the method comprising:

[0007] An insulating layer is fabricated on a metal substrate;

[0008] The insulating layer is patterned to obtain a first microstructure, which includes a plurality of first units arranged in an array.

[0009] Electroplating is performed using the metal substrate as a cathode to form a metal template on the microstructure, the metal template having an array of microgrooves;

[0010] Photoresist is injected into the microgrooves of the metal template and used to cover the substrate structure;

[0011] Remove the metal template to form a second microstructure on the substrate structure. The second microstructure includes a plurality of second units arranged in an array.

[0012] The second microstructure is heated to soften the surface of each second unit of the second microstructure into a spherical shape.

[0013] A transparent filler layer is coated on the second microstructure to obtain a microlens, wherein the transmittance of the transparent filler layer is greater than that of the second microstructure.

[0014] Optionally, the insulating layer is a UV-curable adhesive layer, and the thickness of the insulating layer is 3-5 micrometers.

[0015] Optionally, the step of patterning the insulating layer includes:

[0016] X-rays are used as a light source, and the UV-curable adhesive layer is exposed and developed through a mask.

[0017] Optionally, the first unit is a cuboid, the length of which is 9-10 micrometers and the width of which is 3-4 micrometers.

[0018] Optionally, the metal substrate is a titanium substrate; the method further includes:

[0019] Before forming the insulating layer, the metal substrate is treated with ozone to form a layer of titanium oxide on the surface of the metal substrate.

[0020] Optionally, the electroplating time is 9-10 hours.

[0021] Optionally, heating the second microstructure includes:

[0022] The second microstructure is heated to 105-125 degrees Celsius for 2-5 minutes.

[0023] Optionally, the method further includes:

[0024] After heating the second microstructure, it is annealed at a temperature of 130-160 degrees Celsius.

[0025] Optionally, the method further includes:

[0026] After the transparent filler layer is made, it is baked at a temperature of 65-85 degrees Celsius for 3-4 hours.

[0027] Optionally, the spacing between adjacent second units after softening is 1-2 micrometers, the bottom width of the softened second unit is 3-5 micrometers, and the height of the softened second unit is 2-4 micrometers.

[0028] The beneficial effects of the technical solutions provided in this disclosure are:

[0029] In this embodiment, a reusable metal template is first fabricated through patterning and electroplating processes. This means the metal template fabrication step only needs to be performed once, eliminating the need for repeated steps and subsequent photolithography. This significantly simplifies the fabrication process and enables mass production of microlenses. After the metal template is fabricated, photoresist is applied to cover the substrate structure, resulting in a structure with multiple second units. The structure is then softened by heating to form a hemispherical shape, and finally covered with a transparent filler layer to obtain the microlens formed on the substrate structure. This method eliminates the need for developing and exposing the photoresist on the substrate structure, avoiding corrosion caused by soaking the substrate structure in developing or stripping solutions. This prevents the microlens fabrication from having a fatal impact on the lifespan of the substrate structure. Attached Figure Description

[0030] To more clearly illustrate the technical solutions in the embodiments of this disclosure, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this disclosure. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0031] Figure 1 This is a flowchart of a microlens fabrication method provided in an embodiment of this disclosure;

[0032] Figure 2 This is a flowchart of another microlens fabrication method provided in this embodiment;

[0033] Figure 3 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure;

[0034] Figure 4 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure;

[0035] Figure 5 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure;

[0036] Figure 6 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure;

[0037] Figure 7 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure;

[0038] Figure 8 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure;

[0039] Figure 9This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure;

[0040] Figure 10 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in the embodiments of this disclosure.

[0041] Figure label:

[0042] 301: Metal substrate; 302: UV-curable adhesive layer; 303: X-ray; 304: Mask; 305: First microstructure; 306: Metal template; 307: Photoresist; 308: Substrate structure; 309: Second microstructure; 310: Transparent filler layer. Detailed Implementation

[0043] To make the objectives, technical solutions, and advantages of this disclosure clearer, the embodiments of this disclosure will be described in further detail below with reference to the accompanying drawings.

[0044] Figure 1 This is a flowchart illustrating a microlens fabrication method according to an embodiment of this disclosure. See also... Figure 1 The method includes:

[0045] Step 101: Fabricate an insulating layer on a metal substrate.

[0046] In one possible implementation of this disclosure, the metal substrate is a Ti substrate and the insulating layer is a UV-curable adhesive layer.

[0047] In other possible implementations, the metal substrate and the insulating layer can be made of other materials, and this disclosure does not limit them.

[0048] For example, the thickness of the insulating layer is 3-5 micrometers. For instance, the thickness of the insulating layer is 4 micrometers.

[0049] Step 102: The insulating layer is patterned to obtain the first microstructure.

[0050] The first microstructure includes multiple first units arranged in an array.

[0051] In this embodiment of the disclosure, the patterning process can be etching, such as photolithography, wet etching, dry etching, and other processes.

[0052] In one possible implementation of this disclosure, the insulating layer is a UV-curable adhesive layer. In this case, X-rays can be used to irradiate the UV-curable adhesive layer through a mask to achieve the exposure purpose. The exposed UV-curable adhesive layer is then developed to obtain the first microstructure.

[0053] In other possible implementations of this disclosure, the graphical processing of the insulating layer may also employ other methods.

[0054] In one possible implementation of this disclosure, the first unit is a cuboid.

[0055] In other possible implementations of this disclosure, the first unit may be of other shapes, such as cylindrical, prismatic, etc.

[0056] For example, the first unit is a cuboid with a length of 9-10 micrometers, a width of 3-4 micrometers, and a height of 3-5 micrometers. Of course, the above dimensions are merely an example and are not intended to limit this disclosure.

[0057] Step 103: Electroplating is performed using the metal substrate as a cathode to form a metal template on the microstructure.

[0058] The metal template has an array of micro-grooves, which match the first microstructure. That is, the shape of the groove is consistent with the shape of the first unit, and the distribution of the groove is consistent with the distribution of the first unit.

[0059] In this embodiment of the disclosure, the metal template obtained by electroplating can be a metal template made of nickel, copper, gold, iron-nickel alloy, or the like.

[0060] In this embodiment of the disclosure, the electroplating time is 9-10 hours.

[0061] In this embodiment of the disclosure, the electroplating parameters are as follows: current density is 0.1-1 A / dm³. 2 The electroplating solution is a cyanide electroplating solution for gold plating, with a temperature of 50-80 degrees Celsius and a pH value of 5-7. Of course, the above electroplating time and parameters are merely examples and are not intended to limit this disclosure.

[0062] In this embodiment of the disclosure, the metal template fabrication step only needs to be performed once, that is, steps 101-103 only need to be executed once, and the subsequent fabrication of microlenses only needs to start from step 104.

[0063] The metal template can be reused in subsequent manufacturing processes, making it easy to mass-produce microlenses repeatedly.

[0064] Step 104: Inject photoresist into the micro-grooves of the metal template and cover the substrate structure.

[0065] In one possible implementation of the present disclosure, the substrate structure may be an OLED device, thereby enabling the microlens to be formed on the OLED device.

[0066] In another possible implementation of the embodiments of this disclosure, the substrate structure may also be other structures, such as cover plates or other display devices, optical devices, etc., and this disclosure does not limit them.

[0067] Step 105: Remove the metal template to form a second microstructure on the substrate structure.

[0068] The second microstructure includes multiple second units arranged in an array. The second microstructure matches the micro-grooves on the metal template, that is, the shape of the second unit is consistent with the shape of the groove, and the distribution of the second unit is consistent with the distribution of the groove.

[0069] Step 106: Heat the second microstructure to soften the surface of each second unit of the second microstructure into a spherical shape.

[0070] For example, the second microstructure is heated to 105-125 degrees Celsius for 2-5 minutes.

[0071] It should be noted that, in the embodiments of this disclosure, the second unit is actually similar to a semi-ellipsoid after softening, and is usually not a regular hemisphere or a regular semi-ellipsoid.

[0072] For example, the spacing between adjacent second units after softening is 1-2 micrometers, the bottom width of the softened second unit is 3-5 micrometers, and the height of the softened second unit is 2-4 micrometers.

[0073] The bottom surface of the second unit, after softening, that contacts the substrate structure is elliptical, and the width of the bottom surface refers to the length of the minor axis of the ellipse.

[0074] Of course, the heating parameters and the softened dimensions of the second unit described above are merely examples and are not intended to limit this disclosure.

[0075] Step 107: Cover the second microstructure with a transparent filler layer to obtain a microlens.

[0076] The transmittance of the transparent filler layer is greater than that of the second microstructure.

[0077] In this embodiment of the disclosure, the transparent filler layer can be a high-transmittance adhesive.

[0078] In this embodiment of the disclosure, the high-transmittance adhesive is used only to fill the portions between the individual second units in the second microstructure.

[0079] In this embodiment, a reusable metal template is first fabricated through patterning and electroplating processes. This means the metal template fabrication step only needs to be performed once, eliminating the need for repeated steps and subsequent photolithography. This significantly simplifies the fabrication process and enables mass production of microlenses. After the metal template is fabricated, photoresist is applied to cover the substrate structure, resulting in a structure with multiple second units. The structure is then softened by heating to form a hemispherical shape, and finally covered with a transparent filler layer to obtain the microlens formed on the substrate structure. This method eliminates the need for developing and exposing the photoresist on the substrate structure, avoiding corrosion caused by soaking the substrate structure in developing or stripping solutions. This prevents the microlens fabrication from having a fatal impact on the lifespan of the substrate structure.

[0080] Figure 2 This is a flowchart illustrating a microlens fabrication method according to an embodiment of this disclosure. See also... Figure 2 The method includes:

[0081] Step 201: Treat the titanium metal substrate with ozone to form a layer of titanium oxide on the surface of the metal substrate.

[0082] In this implementation, ozone treatment induces the formation of a titanium oxide layer on the surface of the metal Ti, increasing the surface area and thus increasing adhesion. This prevents the first microstructure from being removed during subsequent development and resist removal processes, ensuring the adhesion of the first microstructure to the metal substrate.

[0083] Step 202: Fabricate a UV-curable adhesive layer on a metal substrate.

[0084] For example, the thickness of the UV-curable adhesive layer is 3-5 micrometers. For instance, the thickness of the UV-curable adhesive layer is 4 micrometers.

[0085] Figure 3 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure. See also... Figure 3 A UV-curable adhesive layer 302 was fabricated on a metal substrate 301.

[0086] Step 203: Using X-rays as a light source, the UV-curable adhesive layer is exposed and developed through a mask to obtain the first microstructure.

[0087] The first microstructure includes multiple first units arranged in an array.

[0088] In this implementation, the first microstructure is fabricated using an ultraviolet-cured adhesive layer, and exposed and developed using X-rays as a light source, which simplifies the fabrication process of the first microstructure.

[0089] In this embodiment of the disclosure, the above-mentioned developing process uses an acidic solution as the developing liquid. During developing, the acidic solution removes the titanium oxide on the exposed surface of the metal substrate, so that the titanium oxide will not affect the subsequent electroplating.

[0090] For example, the first unit is a cuboid with a length of 9-10 micrometers and a width of 3-4 micrometers.

[0091] The height of the cuboid is the thickness of the UV-cured adhesive layer, which is 3-5 micrometers.

[0092] For example, the length of the cuboid is 9 micrometers, the width of the cuboid is 3 micrometers, and the height of the cuboid is 3 micrometers.

[0093] Figure 4 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure. See also... Figure 4 X-rays 303 pass through the mask 304 and irradiate the ultraviolet-cured adhesive layer 302 to achieve the purpose of exposure.

[0094] Figure 5 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure. See also... Figure 5 The UV-cured adhesive layer 302 after exposure is developed to obtain the first microstructure 305.

[0095] Step 204: Electroplating is performed using the metal substrate as a cathode to form a metal template on the microstructure.

[0096] The metal template has an array of micro-grooves.

[0097] In this implementation method, electroplating is used to make metal templates, and the manufacturing process is relatively simple.

[0098] In this embodiment of the disclosure, the metal template obtained by electroplating can be a metal template made of nickel, copper, gold, iron-nickel alloy, or the like.

[0099] For example, the electroplating time is 9-10 hours.

[0100] For example, the electroplating time is 9 hours.

[0101] In this implementation method, electroplating for 9-10 hours can ensure the integrity of the electroplated metal template.

[0102] In this embodiment of the disclosure, the electroplating parameters are as follows: current density is 0.1-1 A / dm³. 2 The electroplating solution is a cyanide electroplating solution for gold plating. The temperature of the electroplating solution is 50-80 degrees Celsius, and the pH value of the electroplating solution is 5-7.

[0103] For example, the electroplating parameters are as follows: current density is 0.5 A / dm². 2 The electroplating solution is a cyanide electroplating solution for gold plating. The temperature of the electroplating solution is 60 degrees Celsius, and the pH value of the electroplating solution is 6.

[0104] In this embodiment of the disclosure, the metal template manufacturing step only needs to be performed once, that is, steps 201-204 only need to be executed once, and the subsequent fabrication of microlenses only needs to start from step 205.

[0105] The metal template can be reused in subsequent manufacturing processes, enabling the microlenses to be easily and repeatedly mass-produced.

[0106] Figure 6 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure. See also... Figure 6 Electroplating is performed on a metal substrate 301 on which the first microstructure 305 is formed to form a metal template 306. The micro grooves on the metal template 306 are matched with the first microstructure 305, that is, the shape of the grooves is consistent with the shape of the first unit, and the distribution of the grooves is consistent with the distribution of the first unit.

[0107] Step 205: Inject photoresist into the micro-grooves of the metal template and cover the substrate structure.

[0108] In one possible implementation of the present disclosure, the substrate structure may be an OLED device, thereby enabling the microlens to be formed on the OLED device.

[0109] In another possible implementation of the embodiments of this disclosure, the substrate structure may also be other structures, such as cover plates or other display devices, optical devices, etc., and this disclosure does not limit them.

[0110] Figure 7 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure. See also... Figure 7 The metal template 306 is separated from the first microstructure 305, and then photoresist 307 is injected into the microgroove of the metal template 306, and then the substrate structure 308 is covered.

[0111] Step 206: Remove the metal template and form a second microstructure on the substrate structure.

[0112] The second microstructure includes multiple second units arranged in an array. The second microstructure matches the micro-grooves on the metal template, that is, the shape of the second unit is consistent with the shape of the groove, and the distribution of the second unit is consistent with the distribution of the groove.

[0113] Figure 8This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure. See also... Figure 8 The metal template 306 is separated to obtain the substrate structure 308 and the second microstructure 309 on the substrate structure 308.

[0114] Step 207: Heat the second microstructure to 105-125 degrees Celsius for 2-5 minutes to soften the surface of each second unit of the second microstructure into a spherical shape.

[0115] For example, the second microstructure is heated to 115 degrees Celsius for 3 minutes.

[0116] In this implementation, the heating time and temperature mentioned above can ensure the softening effect of the second microstructure, so that the surface of each second unit softens into a spherical shape.

[0117] It should be noted that, in the embodiments of this disclosure, the second unit is actually similar to a semi-ellipsoid after softening, and is usually not a regular hemisphere or a regular semi-ellipsoid.

[0118] For example, the spacing between adjacent second units after softening is 1-2 micrometers, the bottom width of the softened second unit is 3-5 micrometers, and the height of the softened second unit is 2-4 micrometers.

[0119] The bottom surface of the second unit, after softening, that contacts the substrate structure is elliptical, and the width of the bottom surface refers to the length of the minor axis of the ellipse.

[0120] For example, the spacing between adjacent second units after softening is 2 micrometers, the bottom width of the softened second unit is 3 micrometers, and the height of the softened second unit is 3 micrometers.

[0121] In this implementation, a second microstructure of the above specifications is formed by heating and softening, thereby obtaining a microlens array.

[0122] Figure 9 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure. See also... Figure 9 The second microstructure 309 on the substrate structure 308 softens after heating, forming a second microstructure 309 with a spherical surface.

[0123] Step 208: After heating the second microstructure, perform annealing treatment at a temperature of 130-160 degrees Celsius.

[0124] For example, the annealing temperature is 150 degrees Celsius.

[0125] In this implementation, the second microstructure is annealed to fix it, thereby forming a microlens array.

[0126] In this embodiment of the disclosure, the annealing time can be several minutes, such as 3 minutes or 5 minutes.

[0127] Step 209: Cover the second microstructure with a transparent filler layer to obtain a microlens.

[0128] The transmittance of the transparent filler layer is greater than that of the second microstructure.

[0129] In this embodiment of the disclosure, the transparent filler layer can be a high-transmittance adhesive.

[0130] In this embodiment of the disclosure, the high-transmittance adhesive is used only to fill the portions between the individual second units in the second microstructure.

[0131] In this implementation, a transparent filler layer is used to provide a basis for the subsequent formation of other structures on the microlens.

[0132] Figure 10 This is a schematic diagram of the microlens structure during the fabrication process of the microlens provided in this embodiment of the disclosure. See also... Figure 10 A transparent filler layer 310 is placed over the second microstructure 309.

[0133] Step 210: After the transparent filler layer is made, the transparent filler layer is baked at a temperature of 65-85 degrees Celsius for 3-4 hours.

[0134] For example, the baking temperature is 75 degrees Celsius and the baking time is 3 hours.

[0135] In this implementation, the transparent filler layer is baked to solidify and set its shape.

[0136] In this embodiment, ozone treatment induces the formation of a titanium oxide layer on the surface of the metal Ti, increasing the surface area and thus increasing adhesion, so as to prevent the first microstructure from being removed during subsequent development and resist removal processes, thereby ensuring the adhesion of the first microstructure to the metal substrate.

[0137] The first microstructure is fabricated using a UV-curable adhesive layer and exposed and developed using X-rays as a light source, which simplifies the fabrication process of the first microstructure.

[0138] Then, an electroplating process is used to create a reusable metal template, so that the metal template making step only needs to be performed once, and there is no need to repeat the metal template making step in the future, thus greatly reducing the production process.

[0139] After the metal template is fabricated, photoresist is introduced and applied to the substrate structure to obtain a structure with multiple second units. Then, the structure is softened by heating to form a hemisphere, and a transparent filler layer is applied to obtain a microlens formed on the substrate structure. This method eliminates the need for developing and exposing the photoresist on the substrate structure, avoiding corrosion caused by soaking the substrate structure in developing or stripping solutions, and preventing the fabrication of microlenses from having a fatal impact on the lifespan of the substrate structure.

[0140] The above description is merely an embodiment of this disclosure and is not intended to limit this disclosure. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this disclosure should be included within the protection scope of this disclosure.

Claims

1. A method for fabricating a microlens, characterized in that, The microlens fabrication method includes: Ozone is used to treat a titanium metal substrate to form a layer of titanium oxide on the surface of the metal substrate; An insulating layer is formed on the metal substrate, and the insulating layer is a UV-curable adhesive layer; Using X-rays as a light source, the UV-curable adhesive layer is exposed and developed through a mask to obtain a first microstructure, which includes multiple first units arranged in an array; the development process uses an acidic solution as the developing solution, which removes the titanium oxide on the exposed surface of the metal substrate during development. Electroplating is performed using the metal substrate as a cathode to form a metal template on the microstructure, the metal template having an array of microgrooves; Photoresist is injected into the microgrooves of the metal template and used to cover the substrate structure, which is an OLED device. Remove the metal template to form a second microstructure on the substrate structure. The second microstructure includes a plurality of second units arranged in an array. The second microstructure is heated to soften the surface of each second unit of the second microstructure into a spherical shape. A transparent filler layer is coated on the second microstructure to obtain a microlens, wherein the transmittance of the transparent filler layer is greater than that of the second microstructure.

2. The microlens fabrication method according to claim 1, characterized in that, The thickness of the insulating layer is 3-5 micrometers.

3. The method for fabricating a microlens according to any one of claims 1 to 2, characterized in that, The first unit is a cuboid, the length of which is 9-10 micrometers and the width of which is 3-4 micrometers.

4. The method for fabricating a microlens according to any one of claims 1 to 2, characterized in that, The electroplating time is 9-10 hours.

5. The method for fabricating a microlens according to any one of claims 1 to 2, characterized in that, The heating of the second microstructure includes: The second microstructure is heated to 105-125 degrees Celsius for 2-5 minutes.

6. The method for fabricating a microlens according to any one of claims 1 to 2, characterized in that, The method further includes: After heating the second microstructure, it is annealed at a temperature of 130-160 degrees Celsius.

7. The method for fabricating a microlens according to any one of claims 1 to 2, characterized in that, The method further includes: After the transparent filler layer is made, it is baked at a temperature of 65-85 degrees Celsius for 3-4 hours.

8. The method for fabricating a microlens according to any one of claims 1 to 2, characterized in that, After softening, the spacing between adjacent second units is 1-2 micrometers, the bottom width of the softened second unit is 3-5 micrometers, and the height of the softened second unit is 2-4 micrometers.

Citation Information

Patent Citations

  • Preparation method of micro-lens array imaging assembly

    CN114913558A