A core-shell structured metal lithium composite material, a preparation method therefor, and use thereof

By designing a core-shell structure in the lithium metal anode material, with the core being lithium metal particles, the middle layer being a lithium deposition-induced layer, and the outer layer being a volume expansion reserved layer, the problems of volume change and dendrite formation in lithium batteries are solved, thereby improving the energy density and cycle life of the battery.

CN117525309BActive Publication Date: 2026-11-24CHINA ENERGY LITHIUM
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210919194.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-29
Publication Date
2026-11-24
Estimated Expiration
2042-07-29

AI Technical Summary

Technical Problem

Existing lithium metal anode materials have problems such as large volume changes and easy dendrite formation in lithium batteries, which affect the energy density and cycle life of the battery.

Method used

A core-shell structured lithium metal composite material is used, with a core of lithium metal particles, a middle layer of lithium deposition induction layer containing lithium-affinity materials, and an outer layer of lithium-repellent volume expansion reserve layer. By controlling the changes in lithium deposition position and volume, dendrite growth is suppressed.

Benefits of technology

It effectively solved the problems of volume change and dendrite formation, improved the energy density and cycle life of the battery, and enhanced structural stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117525309B_ABST
    Figure CN117525309B_ABST
Patent Text Reader

Abstract

This invention provides a core-shell structured lithium metal composite material, its preparation method, and its applications. The lithium metal composite material of this invention uses lithium metal particles as the core, with a lithium deposition-inducing layer containing a lithiophilic material as the intermediate layer and a lithiophore-resistant volume expansion reserve layer as the outermost layer. The composite material provided by this invention, by setting the lithium deposition-inducing layer on the lithium metal particles, can induce preferential deposition and growth of lithium metal inwards, which is beneficial to improving the cycle performance of the composite material. The volume expansion reserve layer provides lithium-ion transport channels while effectively alleviating the volume expansion problem during lithium metal cycling. The lithium deposition-inducing layer and the volume expansion reserve layer work together to significantly improve the cycle life of the composite material, at 1 mA / cm². 2 and 0.5mAh / cm 2 Under certain conditions, it can be stably cycled for more than 400 hours.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of new materials technology, and in particular relates to a core-shell structured metallic lithium composite material, its preparation method, and its applications. Background Technology

[0002] Lithium metal has a theoretical specific capacity of 3860 mAh / g, ten times that of graphite anodes, and a redox potential of -3.04 V vs. standard hydrogen potential, the lowest known among anode materials. Therefore, lithium metal anodes are hailed as the "holy grail" of battery anode materials. Using lithium metal as a battery material can significantly improve battery energy density. However, currently, whether using lithium strips or lithium metal powder as the anode active material, both suffer from large volume changes and a tendency to form dendrites. To address this issue, this application proposes a core-shell structured lithium metal composite material that can provide high energy density while solving the problems of volume changes and dendrite formation during cycling, thereby improving battery energy density and cycle life. Summary of the Invention

[0003] The present invention aims to solve the above-mentioned technical problems. The inventors have discovered that by using lithium metal particles as the core, a lithium deposition-induced layer as the intermediate layer coating the lithium metal particles, and a volume expansion reserved layer as the outermost layer, the core-shell structure of the lithium metal composite material formed can effectively solve the above problems.

[0004] Specifically, one aspect of the present invention provides a core-shell structured lithium metal composite material, wherein the composite material has lithium metal particles as the core, and a lithium deposition induction layer containing lithium-philic materials as an intermediate layer and a lithium-repellent volume expansion reserve layer as the outermost layer are disposed on the core.

[0005] In this invention, a lithium deposition-inducing layer containing lithiophilic materials is incorporated into the composite material to regulate lithium deposition and induce lithium deposition and growth towards the interior; a lithiophore-resistant volume expansion layer regulates lithium ion transport towards the interior, preventing lithium from depositing on the outermost layer. The ingenious design and synergy of the lithiophilic-lithophore-resistant structure of the lithium deposition-inducing layer containing lithiophilic materials and the lithiophore-resistant volume expansion layer effectively solve the problems of volume changes and dendrite formation during cycling, thereby improving the cycling performance of the composite material.

[0006] Optionally, the lithium metal particles may or may not have a protective layer. The protective layer may include, but is not limited to, lithium fluoride, lithium carbonate, polyethylene oxide, polyethylene glycol, polysiloxane, polytrimethylene carbonate, polycarbonate, polyvinyl carbonate, polypropylene carbonate, polyvinyl carbonate, polyvinylidene carbonate, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, poly(vinylidene fluoride-hexafluoropropylene), polyphenylene sulfide, p-benzoquinone, and copolymers or mixtures of at least two of the above polymers.

[0007] Optionally, the average particle size of the lithium metal particles is 1-100 μm, for example, it can be 1 μm.

[0008] 3μm, 5μm, 10μm, 15μm, 20μm, 30μm, 40μm, 45μm, 50μm, 60μm, 70μm, 80μm, 90μm, 95μm or 100μm, etc., preferably 5-50μm.

[0009] Optionally, the lithiophilic material includes lithiophilic nanoparticles, micro / nano carriers loaded with lithiophilic nanoparticles, and / or micro / nano carriers doped with lithiophilic elements.

[0010] In this invention, the lithium deposition induction layer may include lithium-philic nanoparticles and / or lithium-philic elements. The lithium-philic nanoparticles may exist alone on the surface of metallic lithium particles, or they may be attached to micro / nano carriers such as carbon nanotubes, copper nanowires, or graphene and disposed on the surface of metallic lithium particles. 。 The carrier provides support points for the nanoparticles, achieving structural stability, and also supports the volume expansion layer, which helps to further improve the structural stability of the material.

[0011] Optionally, the lithiophilic element includes any one or a combination of at least two of nitrogen, phosphorus, sulfur, boron, fluorine, or oxygen.

[0012] Optionally, the lithium-loving nanoparticles include any one or a combination of at least two of Ag, Au, Sn, Si, Zn, Al, Mg, In, Ga, ZnO, Co3O4, SnS2 or Ni2P, preferably Ag and Au, Ag and Sn, Ag and Mg, Mg and In, Zn and ZnO, etc.

[0013] Optionally, the average particle size of the lithiophilic nanoparticles is 1-200 nm, for example, it can be 1 nm, 2 nm, 4 nm, 5 nm, 7 nm, 9 nm, 10 nm, 15 nm, 20 nm, 50 nm, 70 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 150 nm, 170 nm, 190 nm or 200 nm, etc. If the particle size of the lithiophilic nanoparticles is too small, it is not conducive to uniform distribution; if the particle size is too large, it is not conducive to the formation of a lithium deposition-induced layer. Preferably, it is 5-120 nm, and more preferably 10-100 nm.

[0014] Optionally, the micro / nano carrier includes any one or a combination of at least two of carbon nanotubes, carbon nanofibers, graphene, copper nanowires, Ketjen black, conductive carbon black Super P, porous carbon, fullerene, or conductive graphite, including but not limited to carbon nanotubes and Ketjen black, carbon nanofibers and porous carbon, graphene, conductive carbon black Super P and copper nanowires, fullerene and conductive graphite, etc.

[0015] Optionally, the mass ratio of the lithium deposition induction layer to the lithium metal particles is 1:(1-150), for example, it can be 1:1, 1:2, 1:4, 1:7, 1:10, 1:12, 1:15, 1:18, 1:20, 1:30, 1:50, 1:60, 1:70, 1:90, 1:100, 1:110, 1:130 or 1:150, etc. If the mass ratio is too small, it will not achieve the effect of controlling the deposition of lithium metal; if the mass ratio is too large, it will introduce more inactive substances and reduce the energy density of the material. Preferably, it is 1:(5-120), and more preferably 1:(15-80).

[0016] Optionally, the volume expansion reserved layer comprises one or a combination of at least two structural materials having sheet-like, linear, or tubular micro / nano structures (micron-structures and / or nanostructures), wherein the structural materials include lithium-repellent metals and / or micro / nano carbon materials. The structural materials are interconnected and interwoven during the formation of the volume expansion layer, giving the volume expansion layer a certain rigidity and porosity, facilitating electrolyte wetting and lithium ion transport.

[0017] In this invention, the structural material may be the same as or different from the micro / nano carrier material in the lithium deposition induction layer. For example, the structural material may be any one or a combination of at least two of copper nanowires, carbon nanotubes, carbon nanofibers, or graphene. The micro / nano carrier material of the lithium deposition induction layer may be carbon nanotubes, graphene, fullerenes, Ketjen black, etc., and is not limited by the type of structural material.

[0018] In this invention, lithium-repellent metals and / or carbon materials are selected as the volume expansion reserve layer. While lithium ions can be transported, the deposition of metallic lithium on the surface of the volume expansion reserve layer is suppressed, the growth of lithium dendrites on the surface is suppressed, and the cycle life of the composite material is extended. At the same time, the volume expansion reserve layer has a certain rigidity and porosity, which reserves space for the volume expansion of metallic lithium.

[0019] Optionally, the lithium-phobic metal includes copper nanowires.

[0020] Preferably, the micro / nano carbon material includes carbon nanotubes, carbon nanofibers, and graphene. 、Any one or a combination of at least two of fullerene, Ketjen black, or conductive carbon black Super P. For example, it can be carbon nanotubes and graphene, fullerene and conductive carbon black Super P, carbon nanofibers, graphene, and Ketjen black.

[0021] Optionally, the mass ratio of the volume expansion reserve layer to the lithium metal particles is 1:(1-50), for example, it can be 1:1, 1:2, 1:4, 1:7, 1:10, 1:12, 1:15, 1:18, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45 or 1:50, etc. If the mass ratio is too small, it is not easy to form the volume expansion reserve layer; if the mass ratio is too large, there will be more inactive substances, which is not conducive to improving the energy density of the material. Preferably, it is 1:(12-40).

[0022] Another aspect of the present invention provides a method for preparing the above-described core-shell structured lithium metal composite material, the method comprising:

[0023] (1) Mix organic solvent, lithium metal particles and lithium-loving material, and set the lithium deposition induction layer formed by the lithium-loving material on the lithium metal particles to obtain a precursor;

[0024] (2) The precursor from step (1) is mixed with the structural material, and then spray-dried or stirred at a speed of more than 6000 rpm to set the volume expansion reserve layer formed by the structural material on the precursor to obtain the composite material.

[0025] Optionally, the organic solvent in step (1) includes any one or a combination of at least two of the following: n-hexane, cyclohexane, N-methylpyrrolidone, benzene, p-xylene, carbon tetrachloride, tetrahydrofuran, liquid paraffin, or 1,2-dichloroethane.

[0026] Optionally, the lithium metal particles in step (1) include pure lithium metal particles and / or lithium metal particles containing a protective layer.

[0027] Optionally, the average particle size of the lithium metal particles in step (1) is 1-100 μm, for example, it can be 1 μm, 3 μm, 5 μm, 10 μm, 15 μm, 20 μm, 30 μm, 40 μm, 45 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 95 μm or 100 μm, preferably 5-50 μm.

[0028] Optionally, the lithiophilic material in step (1) includes lithiophilic nanoparticles, micro / nano carriers loaded with lithiophilic nanoparticles and / or micro / nano carriers doped with lithiophilic elements, preferably micro / nano carriers loaded with lithiophilic nanoparticles and / or doped with lithiophilic elements.

[0029] Optionally, the lithiophilic element includes any one or a combination of at least two of nitrogen, phosphorus, sulfur, boron, fluorine, or oxygen.

[0030] Optionally, the lithium-loving nanoparticles include any one or a combination of at least two of Ag, Au, Sn, Si, Zn, Al, Mg, In, Ga, ZnO, Co3O4, SnS2 or Ni2P, preferably Ag and Au, Ag and Sn, Ag and Mg, Mg and In, Zn and ZnO, etc.

[0031] Optionally, the average particle size of the lithium-loving nanoparticles is 10-200 nm, for example, it can be 1 nm, 2 nm, 4 nm, 5 nm, 7 nm, 9 nm, 10 nm, 15 nm, 20 nm, 50 nm, 70 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 150 nm, 170 nm, 190 nm or 200 nm, etc., preferably 20-120 nm;

[0032] Optionally, the mass ratio of the lithiophilic material to the lithium metal particles in step (1) is 1:(1-150), for example, it can be 1:1, 1:2, 1:4, 1:7, 1:10, 1:12, 1:15, 1:18, 1:20, 1:30, 1:50, 1:60, 1:70, 1:90, 1:100, 1:110, 1:130 or 1:150, etc. If the mass ratio is too small, it will not play a role in controlling the deposition of lithium metal; if the mass ratio is too large, more inactive substances will be introduced, reducing the energy density of the material. Preferably, it is 1:(5-120), and more preferably 1:(15-80).

[0033] Optionally, the shape of the structural material in step (2) includes one or a combination of at least two of the following: sheet-like, wire-like, or tubular micro / nanostructures. The structural material includes lithium-repellent metals and / or micro / nano carbon materials (micrometer-scale and / or nanostructures). For example, the structural material can be any one or a combination of at least two of copper nanowires, carbon nanotubes, carbon nanofibers, or graphene. The micro / nano carrier material of the lithium deposition induction layer can be carbon nanotubes, graphene, fullerenes, conductive carbon black Super P, etc., and is not limited by the type of structural material.

[0034] Optionally, the mass ratio of the structural material to the lithium metal particles in step (2) is 1:(1-50), for example, it can be 1:1, 1:2, 1:4, 1:7, 1:10, 1:12, 1:15, 1:18, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45 or 1:50, etc. If the mass ratio is too small, it is not easy to form a volume expansion reserve layer. If the mass ratio is too large, there will be more inactive substances, which is not conducive to improving the energy density of the material. Preferably, it is 1:(12-40).

[0035] Optionally, the spray drying conditions in step (2) include: an inlet air temperature of 180-240℃, such as 180℃, 185℃, 190℃, 195℃, 200℃, 205℃, 215℃ or 220℃, preferably 200-220℃; an outlet air temperature of 90-110℃, such as 90℃, 95℃, 100℃, 105℃ or 110℃, preferably 100-110℃; and an atomization pressure of 0.1-0.5 MPa, such as 0.2 MPa, 0.25 MPa, 0.3 MPa, 0.35 MPa or 0.4 MPa, preferably 0.2-0.4 MPa.

[0036] Optionally, the high-speed stirring speed in step (2) is 6000-15000 rpm, and the time is 0.5-5 min. For example, the speed can be 6000 rpm, 6500 rpm, 7000 rpm, 75000 rpm, 8000 rpm, 8500 rpm, 9000 rpm, 10000 rpm, 11000 rpm, 11500 rpm, 12000 rpm, 12500 rpm, 13000 rpm, 14000 rpm, 14500 rpm, or 15000 rpm, and the time can be 0.5 min, 1 min, 1.5 min, 2 min, 2.5 min, 3 min, 3.5 min, 4 min, 4.5 min, or 5 min, etc. Preferably, the speed is 8000-12000 rpm, and the time is 1-3 min.

[0037] Another aspect of the present invention provides a lithium battery comprising the composite material described in the first aspect above.

[0038] This invention has at least one of the following beneficial technical effects:

[0039] 1. Core-shell structured lithium metal composite materials have a high lithium metal content (lithium metal particle core), which can provide high energy density.

[0040] 2. The lithium deposition induction layer can effectively transport lithium ions and electrons and contains lithium-loving materials, which can effectively adjust the deposition position and uniformity of lithium metal, inhibit the growth of lithium dendrites, regulate the deposition of lithium metal into the interior of the composite material, and at the same time provide support for the volume expansion reserve layer, which is beneficial to the stability of the structure.

[0041] 3. The volume expansion reserved layer has certain rigidity, porosity and lithium-repellency, which can play the role of a three-dimensional protective skeleton while reserving space for lithium metal deposition and volume change. The ingenious design and mutual cooperation of the lithium deposition induction layer and the volume expansion reserved layer effectively extend the cycle life of the composite material.

[0042] 4. The mass production process is simple and easy to implement, and composite materials with different proportions can be prepared by adjustment. Attached Figure Description

[0043] Figure 1 This is a schematic diagram of the structure of the composite material of the present invention;

[0044] Figure 2 The image shows the SEM image of the precursor prepared in step (1) of Example 2.

[0045] Figure 3 for Figure 2 A magnified view of a portion of the image;

[0046] Figure 4 The image shows a SEM image of the core-shell composite material prepared in step (2) of Example 2.

[0047] Figure 5 Battery cycle test curves for Example 2 and Comparative Examples 1, 2 and 3;

[0048] Figure 6 The battery cycle test curves for Comparative Example 1 and Comparative Example 2 are shown.

[0049] Among them, 1-metallic lithium particles, 2-lithium deposition induction layer, and 3-volume expansion reserved layer. Detailed Implementation

[0050] To facilitate understanding of the present invention, the following embodiments are provided. Those skilled in the art should understand that these embodiments are merely illustrative and should not be construed as limiting the scope of the invention.

[0051] An example illustrating the composite material provided by this invention is shown in the schematic diagram below. Figure 1As shown in the diagram, the composite material has a core-shell structure, with lithium metal particles 1 as the core. A lithium deposition induction layer 2 is disposed on the core. This lithium deposition induction layer contains lithiophilic materials, which can regulate the deposition location and uniformity of lithium metal, causing lithium metal to preferentially deposit inside rather than on the outer surface of the composite material, effectively controlling the formation of lithium dendrites and inhibiting their growth. A volume expansion reserve layer 3 is disposed on the lithium deposition induction layer 2. This volume expansion reserve layer is lithiophore-resistant, cannot provide deposition sites for lithium metal, and has a certain degree of rigidity and porosity to provide sufficient space for the volume expansion of lithium metal and dendrite growth. The cooperation between the lithium deposition induction layer 2 and the volume expansion reserve layer 3, i.e., the ingenious arrangement of the lithiophilic-litreophilic structure, effectively regulates the deposition and growth of lithium metal, inhibits the growth of lithium dendrites on the material surface, and significantly extends the cycle life of the composite material.

[0052] Example 1

[0053] This embodiment provides a core-shell structured lithium metal composite material. The composite material includes a lithium metal particle core, wherein the lithium metal particles are pure lithium metal with an average particle size of 5 μm. Tin powder with an average particle size of 100 nm is disposed on the core as a lithium deposition induction layer. Graphene is disposed on the lithium deposition induction layer as a volume expansion reserve layer.

[0054] The method for preparing the composite material includes the following steps:

[0055] (1) Disperse 0.008g of tin powder with an average particle size of 100nm (purchased from Beijing Deco Island Gold) in p-xylene, add 1.2g of lithium metal particles with an average particle size of 5μm, and mechanically stir to set the lithium deposition-induced layer formed by the nano tin powder on the lithium metal particles to obtain the precursor.

[0056] (2) The precursor in step (1) is mixed with 0.8g of graphene dispersion, the mass fraction of graphene in the dispersion is 3%, and the mixture is stirred for 1min at a speed of 8000rpm to obtain the composite material.

[0057] Example 2

[0058] This embodiment provides a core-shell structured lithium metal composite material. The composite material includes a lithium metal particle core, wherein the lithium metal particles are lithium metal particles with a protective LiF layer and an average particle size of 45 μm. The core is provided with single-walled carbon nanotubes with silver powder deposited on it, which serve as a lithium deposition induction layer. The lithium deposition induction layer is provided with single-walled carbon nanotubes as a volume expansion reserve layer.

[0059] The method for preparing the composite material includes the following steps:

[0060] (1) 0.015 g of silver powder with an average particle size of 20 nm (purchased from Xidian Laboratory) and 0.005 g of single-walled carbon nanotube dispersion (purchased from Aokeshier) were dispersed in n-hexane. 1.2 g of lithium metal particles with an average particle size of 45 μm were added, and the mixture was stirred at a high speed of 10000 rpm. A lithium deposition-induced layer formed by single-walled carbon nanotubes with deposited silver powder was then placed on the lithium metal particles, yielding the precursor. Its SEM image is shown below. Figure 2 As shown in the enlarged view, Figure 3 As shown, from Figure 3 The nano-silver powder (particulate matter) can be clearly seen adhering to the single-walled carbon nanotubes, forming a lithium deposition-induced layer;

[0061] (2) The precursor from step (1) was mixed with 1.6 g of single-walled carbon nanotube dispersion (purchased from Oktober), the mass fraction of single-walled carbon nanotubes in the dispersion being 3%. Then, spray drying was performed at an inlet air temperature of 200°C, an outlet air temperature of 100°C, and an atomization pressure of 0.3 MPa to obtain the composite material. Its SEM image is shown below. Figure 4 As shown, from Figure 4 It can be clearly seen that single-walled carbon nanotubes form a volume expansion reserve layer on the outermost layer, and the reserve layer has pores.

[0062] Example 3

[0063] This embodiment provides a core-shell structured lithium metal composite material. The composite material includes a lithium metal particle core, wherein the lithium metal particles are pure lithium metal with an average particle size of 100 μm. Cobalt tetroxide with an average particle size of 200 nm is disposed on the core as a lithium deposition induction layer. Copper nanowires are disposed on the lithium deposition induction layer as a volume expansion reserve layer.

[0064] The method for preparing the composite material includes the following steps:

[0065] (1) 1.2g of cobalt tetroxide (purchased from Aladdin) with an average particle size of 200nm was dispersed in n-hexane, and 1.2g of lithium metal particles with an average particle size of 100μm were added. The mixture was stirred at high speed at a rate of 15000rpm to set the lithium deposition-induced layer formed by nano-cobalt oxide on the lithium metal particles to obtain the precursor.

[0066] (2) The precursor in step (1) was mixed with 80g of copper nanowire dispersion (purchased from Aladdin). The mass fraction of copper nanowires in the dispersion was 1.5%. Then, spray drying was carried out with an inlet air temperature of 240°C, an outlet air temperature of 90°C, and an atomization pressure of 0.5 MPa to obtain the composite material.

[0067] Example 4

[0068] This embodiment provides a core-shell structured lithium metal composite material. The composite material includes a lithium metal particle core, wherein the lithium metal particles are pure lithium metal with an average particle size of 30 μm. Nitrogen-doped carbon nanotubes are disposed on the core as a lithium deposition induction layer, and copper nanowires are disposed on the lithium deposition induction layer as a volume expansion reserve layer.

[0069] The method for preparing the composite material includes the following steps:

[0070] (1) 0.01g of nitrogen-doped carbon nanotubes (purchased from Aladdin) were dispersed in tetrahydrofuran, and 1.2g of lithium metal particles with an average particle size of 80μm were added. The mixture was stirred at a high speed of 12000rpm to set the lithium deposition-induced layer formed by the nitrogen-doped carbon nanotubes on the lithium metal particles to obtain the precursor.

[0071] (2) The precursor in step (1) was mixed with 8g of copper nanowire dispersion (purchased from Aladdin). The mass fraction of copper nanowire in the dispersion was 1.5%. Then, the mixture was stirred at high speed for 3 minutes at a speed of 15000 rpm to obtain the composite material.

[0072] Example 5

[0073] Compared with Example 1, the only difference is that the mass of tin powder is replaced with 0.24g, while the other conditions remain the same.

[0074] Example 6

[0075] Compared with Example 1, the only difference is that the mass of tin powder is replaced with 0.01g, while the other conditions remain unchanged.

[0076] Example 7

[0077] Compared with Example 2, the only difference is that the silver powder is replaced with a mixture of tin powder (average particle size 50nm, purchased from Xidian Laboratory) and silver powder in a mass ratio of 1:1, while the other conditions remain unchanged.

[0078] Example 8

[0079] Compared with Example 1, the only difference is that the mass of the graphene dispersion is replaced with 1.0 g, while the other conditions remain unchanged.

[0080] Example 9

[0081] Compared with Example 1, the only difference is that the mass of the graphene dispersion is replaced with 3.35g, while the other conditions remain unchanged.

[0082] Comparative Example 1

[0083] Compared with Example 2, the only difference is that this comparative example provides lithium metal particles with a protective LiF layer, with an average particle size of 45 μm, and without an intermediate layer and an outermost layer.

[0084] Comparative Example 2

[0085] Compared with Example 2, the only difference is that the composite material provided in this comparative example includes a lithium metal particle core, wherein the lithium metal particles are lithium metal particles with a protective layer of LiF and an average particle size of 45 μm. The core is provided with single-walled carbon nanotubes with silver powder deposited on it as a lithium deposition induction layer, and does not include the volume expansion reserved layer formed by the single-walled carbon nanotubes.

[0086] Comparative Example 3

[0087] Compared with Example 2, the only difference is that the composite material provided in this comparative example includes a lithium metal particle core, wherein the lithium metal particles are lithium metal particles with a protective layer of LiF and an average particle size of 45 μm. The core is provided with a volume expansion reserved layer formed by single-walled carbon nanotubes, but does not include a lithium deposition induction layer of single-walled carbon nanotubes with an average particle size of 20 nm for depositing silver powder.

[0088] Material property testing:

[0089] The materials provided in Examples 1-9 and Comparative Examples 1-3 were directly pressed onto copper foam using a tablet press to prepare electrode sheets. These electrode sheets were then assembled into a symmetrical battery, achieving a voltage of 1 mA / cm². 2 and 0.5mAh / cm 2 Cyclic performance was tested under the specified conditions. The test results are shown in Table 1.

[0090] Table 1

[0091]

[0092]

[0093] The following points can be observed from Table 1:

[0094] (1) By combining Examples 1 and 5-6, adjusting the mass ratio of lithiophilic tin powder to lithium metal particles can further optimize the cycle performance of the composite material.

[0095] (2) By combining Examples 1 and 8-9, the mass ratio of graphene to lithium powder in the structural material can be adjusted to further optimize the cycle performance of the composite material.

[0096] (3) The core-shell composite material prepared in Example 2 exhibits better cycling performance than the materials in Comparative Examples 1-3. This is because the lithium deposition-inducing layer in the composite material prepared in Example 2 effectively regulates the deposition location and uniformity of metallic lithium, while the volume expansion reserve layer provides sufficient space for the volume expansion and dendrite growth of metallic lithium. The two work together to significantly improve the cycle life of the composite material. Combining the cycling test curves of Example 2 and Comparative Examples 1-3 (e.g.) Figure 5 and Figure 6 As shown in the figure, the short circuit phenomenon in Comparative Example 2 may be due to the lack of a volume expansion pre-reserved layer. The silver powder controls the preferential deposition of metallic lithium on the outer surface of the composite material, and lithium dendrites are formed as the cycle progresses. The phenomenon of a sharp increase in voltage and resistance in Comparative Example 3 may be due to the lack of a lithium deposition induction layer. As the cycle progresses, the material structure changes.

[0097] Based on the disclosure and teachings of the foregoing specification, those skilled in the art can make appropriate changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the present invention should also fall within the protection scope of the claims of the present invention. Furthermore, although some specific terms are used in this specification, these terms are only for convenience of explanation and do not constitute any limitation on the present invention.

Claims

1. A core-shell structured lithium metal composite material, characterized in that, The composite material has lithium metal particles as its core, with a lithium deposition-inducing layer containing lithiophilic materials as the intermediate layer and a lithiophore-resistant volume expansion reserve layer as the outermost layer. The average particle size of the lithium metal particles is 1-100 μm, and The lithiophilic material includes lithiophilic nanoparticles, micro / nano carriers loaded with lithiophilic nanoparticles, and / or micro / nano carriers doped with lithiophilic elements; the volume expansion reserved layer includes one or a combination of at least two of the structural materials having sheet-like, linear, or tubular micro / nano structures.

2. The composite material according to claim 1, characterized in that, The lithium metal particles may or may not have a protective layer.

3. The composite material according to claim 1, characterized in that, The average particle size of the lithium metal particles is 5-50 μm.

4. The composite material according to claim 1, characterized in that, The lithiophilic element includes any one or a combination of at least two of the elements nitrogen, phosphorus, sulfur, boron, fluorine, or oxygen.

5. The composite material according to claim 1, characterized in that, The lithiophilic nanoparticles include any one or a combination of at least two of Ag, Au, Sn, Si, Zn, Al, Mg, In, Ga, ZnO, Co3O4, SnS2, or Ni2P.

6. The composite material according to claim 1, characterized in that, The average particle size of the lithiophilic nanoparticles is 10-200 nm.

7. The composite material according to claim 1, characterized in that, The micro / nano carriers include any one or a combination of at least two of the following: carbon nanotubes, carbon nanofibers, graphene, copper nanowires, Ketjen black, conductive carbon black Super P, porous carbon, fullerene, or conductive graphite.

8. The composite material according to claim 1, characterized in that, The mass ratio of the lithium deposition-induced layer to the lithium metal particles is 1:(1-150).

9. The composite material according to claim 1, characterized in that, The structural materials include lithium-repellent metals and / or micro / nano carbon materials.

10. The composite material according to claim 9, characterized in that, The lithium-repellent metal includes copper nanowires.

11. The composite material according to claim 9, characterized in that, The micro / nano carbon materials include any one or a combination of at least two of carbon nanotubes, carbon nanofibers, graphene, fullerene, Ketjen black, or conductive carbon black Super P.

12. The composite material according to claim 1, characterized in that, The mass ratio of the volume expansion reserved layer to the lithium metal particles is 1:(1-50).

13. A method for preparing the composite material according to any one of claims 1-12, characterized in that, The method includes: (1) Mix organic solvent, lithium metal particles and lithium-loving material, and set the lithium deposition-inducing layer formed by the lithium-loving material on the lithium metal particles to obtain a precursor; (2) The precursor in step (1) is mixed with the structural material, and then spray-dried or stirred at a speed of more than 6000 rpm to set the volume expansion reserve layer formed by the structural material on the precursor to obtain the composite material.

14. The method according to claim 13, characterized in that, The organic solvent in step (1) includes any one or a combination of at least two of the following: n-hexane, cyclohexane, N-methylpyrrolidone, benzene, p-xylene, carbon tetrachloride, tetrahydrofuran, liquid paraffin, or 1,2-dichloroethane.

15. The method according to claim 13 or 14, characterized in that, The mass ratio of the structural material to the lithium metal particles in step (2) is 1:(1-50).

16. A lithium battery, characterized in that, The lithium battery comprises a composite material as described in any one of claims 1-12.

Citation Information

Patent Citations

  • Lithium anode particle and preparation thereof, and application of lithium anode particle in preparation of lithium anode and lithium battery

    CN111653733A