Composite positive electrode material, preparation method thereof, positive electrode sheet and lithium ion battery

By coating lithium magnesium phosphate onto lithium cobalt oxide and ternary materials to form a core-shell structured composite cathode material, the problem of structural instability of lithium cobalt oxide under high voltage is solved, and a lithium-ion battery with high energy density, long cycle life and safety is realized.

CN117525340BActive Publication Date: 2026-11-20TIANJIN B&M SCI & TECH LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311578190.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-23
Publication Date
2026-11-20
Estimated Expiration
2043-11-23

AI Technical Summary

Technical Problem

Traditional lithium cobalt oxide cathode materials are structurally unstable under high voltage, leading to decreased battery performance, safety hazards, and high cost.

Method used

The composite cathode material is adopted, with a core-shell structure consisting of lithium cobalt oxide and ternary materials as the core and lithium magnesium phosphate as the shell. The core-shell structure is formed by coating with lithium magnesium phosphate through a sol-gel method, which enhances the stability and safety of the material.

Benefits of technology

It improves the energy density and cycle life of lithium-ion batteries at high voltages, reduces cobalt leaching and gas production, enhances battery safety and cycle stability, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117525340B_ABST
    Figure CN117525340B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of lithium ion batteries, in particular to a composite positive electrode material, a preparation method thereof, a positive electrode sheet and a lithium ion battery. The composite positive electrode material has a core-shell structure, the inner core of the core-shell structure comprises a lithium cobaltate material and a ternary material; the ternary material comprises a lithium nickel cobalt manganese oxide material and / or a lithium nickel cobalt aluminum oxide material; and the outer shell of the core-shell structure comprises a lithium magnesium phosphate. The lithium ion battery containing the composite positive electrode material has high capacity and excellent cycle stability at high voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, and more specifically, to a composite cathode material and its preparation method, a cathode sheet, and a lithium-ion battery. Background Technology

[0002] With the rapid development of the lithium-ion battery industry, end products are placing increasingly higher demands on lithium-ion batteries. Since the performance of lithium-ion batteries is primarily determined by the cathode material, the quality of the cathode material has a significant impact on the final performance of the lithium-ion battery. Therefore, the key to developing lithium-ion batteries with high energy density and long cycle life lies in improving the electrochemical performance of the cathode material.

[0003] Lithium cobalt oxide, as a widely used cathode material for lithium-ion batteries, boasts mature production processes and excellent performance. However, traditional lithium cobalt oxide cathode materials experience bulk structure collapse, oxygen evolution, Co dissolution, and surface corrosion during high-voltage charging and discharging, leading to decreased battery performance, rapid capacity decay, and even safety accidents. This severely hinders the application of lithium cobalt oxide cathode materials at high voltages.

[0004] In view of this, the present invention is hereby proposed. Summary of the Invention

[0005] The primary objective of this invention is to provide a composite cathode material that exhibits good structural stability under high voltage, and lithium-ion batteries made using this composite cathode material possess high capacity or excellent cycle stability.

[0006] The second objective of this invention is to provide a method for preparing composite cathode materials that is simple, easy to mass-produce, low in cost, and environmentally friendly.

[0007] A third objective of this invention is to provide a positive electrode sheet comprising the above-mentioned composite positive electrode material.

[0008] A fourth objective of the present invention is to provide a lithium-ion battery comprising the above-described positive electrode.

[0009] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted:

[0010] This invention provides a composite cathode material having a core-shell structure, wherein the core of the core-shell structure comprises lithium cobalt oxide material and a ternary material; wherein the ternary material comprises lithium nickel cobalt manganese oxide material and / or lithium nickel cobalt aluminum oxide material;

[0011] The outer shell of the core-shell structure comprises lithium magnesium phosphate.

[0012] The present invention further provides a method for preparing the composite cathode material, comprising the following steps:

[0013] Lithium cobalt oxide material, ternary material, phosphorus source, magnesium source, lithium source, dispersant and solvent are mixed and subjected to sol-gel reaction to obtain gel;

[0014] The gel is subjected to a first sintering and a second sintering, and then cooled to obtain the composite cathode material.

[0015] The present invention also provides a positive electrode sheet, comprising the composite positive electrode material as described above.

[0016] The present invention also provides a lithium-ion battery, including the positive electrode sheet as described above.

[0017] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0018] (1) The composite cathode material provided by the present invention has a core-shell structure with lithium cobalt oxide and ternary materials as the core and lithium magnesium phosphate as the shell. The battery containing the composite cathode material has high energy density and cycle life under high voltage and has high safety performance.

[0019] (2) The composite cathode material provided by the present invention uses the sol-gel method to coat lithium cobalt oxide material and ternary material with lithium magnesium phosphate sol-gel, which can not only enhance the uniformity of coating, avoid direct contact between lithium cobalt oxide material and ternary material and electrolyte, and reduce the occurrence of side reactions, but also improve the structural stability of composite cathode material under high voltage and reduce cobalt dissolution and gas generation.

[0020] (3) The composite cathode material provided by the present invention combines large-particle-size lithium cobalt oxide material and small-particle-size ternary material to form a core. Compared with a single lithium cobalt oxide core material, it can combine the advantages of both lithium cobalt oxide and ternary material to achieve high specific capacity, high voltage, and excellent tap density and compaction density characteristics. Attached Figure Description

[0021] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0022] Figure 1 SEM image of the composite cathode material prepared in Example 1 of this invention. Detailed Implementation

[0023] The technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings and specific embodiments. However, those skilled in the art will understand that the embodiments described below are some embodiments of the present invention, but not all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall be followed. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0024] Unless otherwise specified, in this invention, terms such as "first aspect," "second aspect," "third aspect," and "fourth aspect" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, terms such as "first," "second," "third," and "fourth" serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on quantity.

[0025] Unless otherwise specified, the terms "comprising" and "including" as used in this invention can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.

[0026] Unless otherwise specified, in this invention, "one or more" or "at least one" refers to any one, any two, or any two or more of the listed items. "Several" refers to any two or more.

[0027] In a first aspect, the present invention provides a composite cathode material having a core-shell structure, wherein the core of the core-shell structure comprises lithium cobalt oxide material and ternary material.

[0028] The ternary material includes lithium nickel cobalt manganese oxide material and / or lithium nickel cobalt aluminum oxide material.

[0029] It is understandable that the core material of a core-shell structure can contain lithium cobalt oxide and lithium nickel cobalt manganese oxide, or it can contain lithium cobalt oxide and lithium nickel cobalt aluminum oxide, or it can contain lithium cobalt oxide, lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide at the same time.

[0030] The outer shell of the core-shell structure is made of lithium magnesium phosphate.

[0031] The composite cathode material provided by this invention has a core-shell structure with lithium cobalt oxide and ternary materials as the core and lithium magnesium phosphate as the shell. Batteries containing this composite cathode material exhibit high energy density and cycle life at high voltages, while also demonstrating good safety and promising application prospects. Specifically, compared to lithium cobalt oxide, ternary materials are inexpensive, have excellent cycle performance, and higher capacity, but their processing performance, compaction density, and voltage plateau are slightly lower than those of lithium cobalt oxide. Mixing the two in a certain proportion can not only improve the overcharge resistance of lithium cobalt oxide materials but also improve the rate performance and energy density of ternary materials.

[0032] Meanwhile, the strong PO covalent bonds in the lithium magnesium phosphate crystal structure of the shell stabilize oxygen atoms when the battery is fully charged, preventing them from being oxidized and releasing oxygen. Simultaneously, Mg doping enhances the ionicity of the cobalt-oxygen bonds, promoting oxygen ion stability. These two factors work together to significantly improve the safety and lifespan of the composite cathode material.

[0033] In some specific embodiments, in order to further improve the capacity and cycle performance of the resulting composite material, the lithium cobalt oxide material includes lithium cobalt oxide and E element doped in the lithium cobalt oxide, wherein E includes at least one of Ca, Sr, Ga, Ge, In, Mg, Al and transition metal elements.

[0034] Further, the aforementioned transition metal element includes at least one selected from Sc, Ti, V, Cr, Mn, Fe, Ni, Cu, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, La, Hf, Ta, W, Re, Os, Ir, Pt, and Au; even further, the transition metal element is preferably at least one selected from Ti, V, Cr, Mn, Fe, Ni, Y, Zr, Nb, and W.

[0035] Among them, E, as a doping element, can regulate the defects and their distribution inside lithium cobalt oxide particles, thereby suppressing the structural phase transition that causes the electrochemical performance of lithium cobalt oxide materials to degrade during high-voltage charge and discharge.

[0036] It is understood that the aforementioned lithium cobalt oxide material can be any commercially available lithium cobalt oxide material or any lithium cobalt oxide material obtained according to any existing technology.

[0037] In some specific embodiments, to further improve the capacity and cycle performance of the obtained composite material, the lithium nickel cobalt manganese oxide material includes lithium nickel cobalt manganese oxide and an element A doped within the lithium nickel cobalt manganese oxide, wherein A includes at least one selected from Ca, Sr, Ga, Ge, In, Mg, Al, and transition metal elements. The lithium nickel cobalt aluminum oxide material includes lithium nickel cobalt aluminum oxide and an element Q doped within the lithium nickel cobalt aluminum oxide, wherein Q includes at least one selected from Ca, Sr, Ga, Ge, In, Mg, Al, and transition metal elements.

[0038] The transition metal elements include at least one of Sc, Ti, V, Cr, Fe, Cu, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, La, Hf, Ta, W, Re, Os, Ir, Pt, and Au.

[0039] Among them, A and Q, as doping elements, can improve the electronic conductivity and ionic conductivity of ternary materials, increase the output power density of batteries, and simultaneously improve the stability of the ternary material structure.

[0040] In some specific embodiments, in order to further improve the electrochemical performance of the ternary material, A includes at least one of Y, W, Ce, Zr, Sr, Ca, Ti and Gd.

[0041] In some specific embodiments, in order to further improve the electrochemical performance of the ternary material, Q includes at least one of Y, W, Ce, Zr, Sr, Ca, Ti and Gd.

[0042] In some specific embodiments, to further improve the capacity and cycle performance of lithium-ion batteries containing composite cathode materials, the E element doping amount in the lithium cobalt oxide material is 100–20000 ppm; including but not limited to any one of 100 ppm, 200 ppm, 300 ppm, 500 ppm, 800 ppm, 900 ppm, 1000 ppm, 3000 ppm, 5000 ppm, 10000 ppm, 15000 ppm, and 20000 ppm, or a range between any two. The A element doping amount in the lithium nickel cobalt manganese oxide material is 100–9000 ppm; including but not limited to any one of 100 ppm, 200 ppm, 300 ppm, 500 ppm, 800 ppm, 900 ppm, 1000 ppm, 3000 ppm, 5000 ppm, 7000 ppm, and 9000 ppm, or a range between any two. The doping amount of Q element in the lithium nickel cobalt aluminum oxide material is 100–9000 ppm; including but not limited to any one of 100 ppm, 200 ppm, 300 ppm, 500 ppm, 800 ppm, 900 ppm, 1000 ppm, 3000 ppm, 5000 ppm, 7000 ppm, and 9000 ppm, or a range between any two. Wherein, ppm refers to mass fraction, and 1 ppm = 1 / 1,000,000.

[0043] It is understood that the aforementioned ternary materials can be any commercially available ternary material or any ternary material obtained according to any existing technology.

[0044] In some specific embodiments, the composite cathode material provided by the present invention has a suitable specific surface area, which is beneficial to improving the capacity, initial coulombic efficiency, and cycle performance of lithium-ion batteries prepared therefrom. The specific surface area of ​​the composite cathode material is 0.17–0.24 m². 2 / g; including but not limited to 0.17m 2 / g, 0.19m 2 / g, 0.20m 2 / g, 0.21m 2 / g, 0.22m 2 / g, 0.23m 2 / g, 0.24m 2 The point value of any one of / g or the range value between any two.

[0045] In some specific embodiments, the composite cathode material provided by the present invention has a suitable tap density, which is beneficial for further improving the capacity, initial coulombic efficiency, and cycle performance of lithium-ion batteries prepared therefrom. The tap density of the composite cathode material is 2.8–3.2 g / cm³. 3; including but not limited to 2.8g / cm 3 2.9g / cm 3 3.0g / cm 3 3.1g / cm 3 3.2g / cm 3 The point value of any one of them or the range value between any two.

[0046] In some specific embodiments, the composite cathode material provided by the present invention has a suitable compaction density, which can further improve the electrochemical performance of lithium-ion batteries prepared therefrom. The compaction density of the composite cathode material is 3.8–4.3 g / cm³. 3 ; including but not limited to 3.8g / cm 3 3.9g / cm 3 4.0g / cm 3 4.3g / cm 3 The point value of any one of them or the range value between any two.

[0047] In some specific embodiments, the median particle size D50 of the composite cathode material is 13 to 17 μm, including but not limited to the point value of any one of 13 μm, 14 μm, 15 μm, 16 μm, and 17 μm, or the range between any two.

[0048] In some specific embodiments, in order to further improve the electrochemical performance of the battery containing the composite cathode material, the mass of the lithium magnesium phosphate is 0.01% to 5% of the total mass of the composite cathode material; including but not limited to any one of 0.01%, 0.05%, 0.1%, 0.3%, 0.5%, 0.8%, 1%, 2%, 3%, 4%, and 5%, or any range between two of them.

[0049] In some specific embodiments, the lithium-ion battery containing the composite cathode material has a first charge specific capacity of 216 to 225 mAh / g at 0.1C, including but not limited to any one of 216 mAh / g, 217 mAh / g, 218 mAh / g, 219 mAh / g, 220 mAh / g, 221 mAh / g, 222 mAh / g, 223 mAh / g, 224 mAh / g, and 225 mAh / g, or a range between any two.

[0050] In some specific embodiments, the lithium-ion battery containing the composite cathode material has an initial discharge specific capacity of 194.5 to 206 mAh / g at 0.1C, including but not limited to any one of 194.5 mAh / g, 196 mAh / g, 198 mAh / g, 200 mAh / g, 202 mAh / g, 204 mAh / g, and 206 mAh / g, or a range between any two.

[0051] In some specific embodiments, the lithium-ion battery containing the composite cathode material has an initial coulombic efficiency of 89.8% to 93.0% at 0.1C, including but not limited to any one of 89.8%, 90%, 91.0%, 92.0%, and 93.0%, or a range between any two.

[0052] In some specific embodiments, the capacity retention rate of a lithium-ion battery containing the composite cathode material after 50 cycles at 45°C is 85.4% to 92.2%, including but not limited to any one of 85.4%, 86.0%, 88.0%, 90.0%, and 92.2%, or a range between any two.

[0053] In some specific embodiments, the reaction time of the sol-gel method is 6 to 8 hours; including but not limited to the point value of any one of 6 hours, 6.5 hours, 7 hours, 7.5 hours, and 8 hours, or the range between any two.

[0054] By using the above reaction temperature and reaction time, the added lithium, magnesium, and phosphorus sources can be fully contacted within a suitable time range, laying a good foundation for subsequent drying and sintering into lithium magnesium phosphate.

[0055] In some specific embodiments, in order to further improve the electrical performance of the battery containing the composite cathode material, the mass ratio of the lithium cobalt oxide material to the ternary material is 6-10:2-5, including but not limited to any one of the following values ​​or any range between two: 6:2, 7:2, 8:2, 9:2, 10:2, 6:3, 7:3, 8:3, 9:3, 10:3, 6:4, 7:4, 8:4, 9:4, 10:4, 6:5, 7:5, 8:5, 9:5, 10:5.

[0056] Secondly, the present invention provides a method for preparing the composite cathode material as described above, comprising the following steps:

[0057] The lithium cobalt oxide material, ternary material, phosphorus source, magnesium source, lithium source, dispersant and solvent are mixed evenly and subjected to sol-gel reaction. After the reaction is completed, a gel is obtained.

[0058] In some specific implementations, the phosphorus source, magnesium source, lithium source, dispersant and solvent are first mixed evenly, and then lithium cobalt oxide material and ternary material are added to it.

[0059] In some specific embodiments, the solvent includes, but is not limited to, water, preferably deionized water.

[0060] It is understandable that the phosphorus source mentioned above refers to compounds containing phosphate.

[0061] The gel is then subjected to a first sintering and a second sintering, and after cooling, the composite cathode material is obtained.

[0062] The method for preparing composite cathode materials provided by this invention, by coating lithium cobalt oxide and ternary materials with lithium magnesium phosphate sol-gel, can not only enhance the uniformity of coating and avoid direct contact between lithium cobalt oxide and ternary materials and electrolyte, thus reducing the occurrence of side reactions, but also improve the structural stability of composite cathode materials under high voltage, reduce cobalt dissolution and gas generation. In this way, under the synergistic effect of the above three types of materials, the shortcomings of single cathode active materials are overcome, and the energy density, cycle life and safety of lithium-ion batteries are improved.

[0063] Furthermore, the above preparation method has the advantages of being simple and easy to implement, having a short process cycle, being energy-saving, easy to mass-produce, having low cost, and being environmentally friendly.

[0064] In some specific embodiments, a drying step is also included before sintering.

[0065] As an example, the drying temperature can be 100–120°C, but is not limited to this.

[0066] In some specific embodiments, after sintering, a crushing and sieving step is also included.

[0067] In the above preparation process, the dispersant plays the role of both a dispersant and a template agent, and can also control the concentration of metal ions.

[0068] In some specific embodiments, the dispersant includes at least one selected from ammonia, ammonium chloride, ammonium sulfate, ammonium carbonate, citric acid, and tartaric acid.

[0069] In some specific embodiments, the molar ratio of dispersant to lithium source is 0.8 to 1.2:1, including but not limited to any one of 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1 or any range between the two.

[0070] In some specific embodiments, the median particle size D50 of the lithium cobalt oxide material is 14 to 20 μm; including but not limited to point values ​​of any one of 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, and 20 μm, or range values ​​between any two.

[0071] In some specific embodiments, the median particle size D50 of the ternary material is 3 to 8 μm; including but not limited to point values ​​of any one of 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, and 8 μm, or range values ​​between any two.

[0072] This invention combines large-particle-size lithium cobalt oxide with small-particle-size ternary materials to obtain a core layer material. Compared to a single lithium cobalt oxide core layer material, this method combines the advantages of both lithium cobalt oxide and ternary materials, resulting in high specific capacity, high voltage, and excellent tap and compaction density characteristics. Simultaneously, the shell layer offers advantages such as high safety performance, long cycle life, and low cost. Therefore, the composite cathode material provided by this invention, after forming a battery, possesses advantages such as high specific capacity, long cycle life, high safety performance, and low cost.

[0073] In some specific embodiments, during the sol-gel reaction, the temperature of the mixture is 60-80°C; including but not limited to any one of 60°C, 65°C, 70°C, 75°C, and 80°C, or any range between two of them.

[0074] In some specific embodiments, the sol-gel reaction is carried out in a water bath at a temperature of 60–80°C, which is beneficial for uniform coating.

[0075] In some specific embodiments, the sol-gel reaction time is 6 to 8 hours; including but not limited to the point value of any one of 6 hours, 6.5 hours, 7 hours, 7.5 hours, and 8 hours, or the range between any two.

[0076] In some specific embodiments, in order to further improve the electrical performance of the composite cathode material, the mass ratio of the lithium cobalt oxide material to the ternary material is 6-10:2-5, including but not limited to any one of the following values ​​or any range between two: 6:2, 7:2, 8:2, 9:2, 10:2, 6:3, 7:3, 8:3, 9:3, 10:3, 6:4, 7:4, 8:4, 9:4, 10:4, 6:5, 7:5, 8:5, 9:5, 10:5.

[0077] In some specific embodiments, the sintering temperature of the gel is relatively low. Specifically, the first sintering temperature is 400–600°C, including but not limited to a value of any one of 400°C, 500°C, and 600°C, or a range between any two. The second sintering temperature is 700–900°C, including but not limited to a value of any one of 700°C, 800°C, and 900°C, or a range between any two.

[0078] In the preparation process, the present invention performs low-temperature sintering on the gel of lithium magnesium phosphate-coated lithium cobalt oxide material and ternary material, which can improve the processing performance of composite cathode material and ensure consistency and stability in battery preparation.

[0079] In some specific embodiments, the first sintering time is 1 to 4 hours; including but not limited to any one of 1 hour, 2 hours, 3 hours, and 4 hours, or any range between two of them.

[0080] In some specific embodiments, the second sintering time is 1 to 4 hours; including but not limited to any one of 1 hour, 2 hours, 3 hours, and 4 hours, or any range between two of them.

[0081] In some specific embodiments, the lithium cobalt oxide material is mainly prepared by mixing a lithium source, a cobalt source, and an E-containing compound, followed by a two-stage calcination process. The E-containing compound includes at least one of Ca, Sr, Ga, Ge, In, Mg, Al, and transition metal elements.

[0082] In some specific embodiments, the preparation method of the lithium cobalt oxide material specifically includes the following steps: mixing a lithium source, a cobalt source and an E-containing compound evenly, then performing a two-stage calcination, cooling and crushing to obtain the lithium cobalt oxide material.

[0083] The lithium source includes any lithium-containing compound, and the cobalt source includes any cobalt-containing compound.

[0084] As an example, lithium sources include, but are not limited to, one or more of lithium carbonate, lithium nitrate, lithium acetate, lithium hydroxide, lithium oxide, lithium chloride, lithium bromide, and lithium fluoride.

[0085] As an example, cobalt sources include one or more of cobalt tetroxide, cobalt hydroxide, cobalt sulfide, cobalt nitrate, cobalt sulfate, and cobalt hydroxyoxide.

[0086] In some specific implementations, the molar ratio of lithium in the lithium source to cobalt in the cobalt source is 1 to 1.1:1.

[0087] In some specific embodiments, the preparation method of the ternary material includes the following steps: mixing the precursor material and the lithium source uniformly, sintering, cooling, and then crushing to obtain the ternary material. Optionally, during the mixing process, the raw materials also include a compound containing A and / or a compound containing Q.

[0088] It is understandable that "optional" means optional or not optional.

[0089] The aforementioned precursor materials include nickel cobalt manganese hydroxide and / or nickel cobalt aluminum hydroxide.

[0090] As an example, nickel-cobalt-manganese hydroxide includes Ni 0.6 Co 0.2 Mn 0.2 (OH)2, Ni 0.8 Co 0.1 Mn 0.1 (OH)2, but not limited to this.

[0091] As an example, nickel-cobalt-aluminum hydroxide includes Ni 0.6 Co 0.2 Al 0.2 (OH)2, Ni 0.8 Co 0.1 Al 0.1 (OH)2, but not limited to this.

[0092] In some specific implementations, during the preparation of ternary materials, the precursor material is first heated to form an oxide from the hydroxide, and then mixed with a lithium source, an A-containing compound, or a Q-containing compound.

[0093] Because the precursor contains moisture and impurities, the actual metal content is lower than the theoretical metal content. Therefore, the oxide precursor formed after heat treatment has a higher metal content than the hydroxide because its molecular formula has changed. In addition, preheating the precursor facilitates subsequent sintering, which in turn improves the electrochemical performance of the ternary material.

[0094] In some specific implementations, the molar ratio of lithium element in the lithium source to the precursor material is 1 to 1.05:1, for example, 1:1, 1.01:1, 1.02:1, 1.03:1, 1.04:1 or 1.05:1.

[0095] In some specific embodiments, the sintering temperature for preparing ternary materials is 500–900°C, for example, 500°C, 600°C, 700°C, 800°C, or 900°C; the holding time for sintering ternary materials is 5–18 hours, for example, 5 hours, 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 15 hours, or 18 hours.

[0096] In some specific embodiments, the ternary material includes lithium nickel cobalt manganese oxide material and lithium nickel cobalt aluminum oxide material with a mass ratio of 1 to 5:0 to 1, wherein the mass ratio can be selected, for example, 1:0, 1:0.3, 2:1, 3:1, 4:1 or 5:1.

[0097] In some specific embodiments, the two-stage calcination specifically includes: firstly, holding at 400-900℃ for 3-8 hours for the first stage of calcination, and then holding at 950-1200℃ for 5-12 hours for the second stage of calcination.

[0098] In the two-stage calcination process, low-temperature calcination is used first, followed by high-temperature calcination, which can make the particle structure of the obtained lithium cobalt oxide material more stable, and thus the composite cathode material prepared has better performance.

[0099] The temperature of the first calcination stage includes, but is not limited to, any one of 400℃, 500℃, 600℃, 700℃, 800℃, and 900℃, or any range between any two. The holding time of the first calcination stage includes, but is not limited to, any one of 3h, 4h, 5h, 6h, 7h, and 8h, or any range between any two.

[0100] The temperature of the second stage of calcination includes, but is not limited to, any one of 950℃, 1000℃, 1050℃, 1100℃, 1150℃, and 1200℃, or any range between two of them. The holding time of the second stage of calcination includes, but is not limited to, any one of 5h, 6h, 7h, 8h, 9h, 10h, 11h, and 12h, or any range between two of them.

[0101] In some specific implementations, the heating rate during the two-stage calcination process is 2 to 10 °C / min, including but not limited to any one of 2 °C / min, 3 °C / min, 5 °C / min, 7 °C / min, 9 °C / min, and 10 °C / min, or any range between two of them.

[0102] In some specific implementations, in order to further improve the structural stability of lithium cobalt oxide materials, the heating rate in the first calcination process is 2 to 10 °C / min, and the heating rate in the second calcination process is 2 to 5 °C / min.

[0103] In some specific implementations, the magnesium source used in the preparation of the composite cathode material includes any magnesium-containing compound.

[0104] As an example, magnesium sources include, but are not limited to, one or more of magnesium phosphate, magnesium nitrate, and magnesium sulfate.

[0105] In some specific implementations, the phosphorus source used in the preparation of the composite cathode material includes any phosphate-containing compound.

[0106] As an example, phosphorus sources include, but are not limited to, one or more of phosphoric acid, ammonium phosphate, sodium phosphate, potassium phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, dipotassium hydrogen phosphate, and potassium dihydrogen phosphate.

[0107] In some specific embodiments, during the preparation of the composite cathode material, the molar ratio of lithium in the lithium source, magnesium in the magnesium source, and phosphorus in the phosphorus source is 1:(0.8~1.3):(0.9~1.2), for example 1:0.8:0.9, 1:0.8:1, 1:0.8:1.1, 1:0.8:1.2, 1:1:0.9, 1:1:1, 1:1:1.1, 1:1:1.2, 1:1.2:0.9, 1:1.2:1, 1:1.2:1.1, or 1:1.3:1.2.

[0108] In some specific embodiments, the calcination, sintering, or drying described in this invention can all be carried out in conventional calcination equipment, such as muffle furnaces, tunnel furnaces, roller kilns, tube furnaces, or other types of calcination equipment. This invention does not impose any limitations.

[0109] Thirdly, the present invention provides a positive electrode sheet comprising the composite positive electrode material as described above.

[0110] In some specific embodiments, the positive electrode sheet includes a current collector and a positive electrode material coated on the current collector, wherein the positive electrode material includes a composite positive electrode material.

[0111] In some specific implementations, the current collector used for the positive electrode can be a metal foil or a composite current collector. For example, the metal foil can be aluminum foil, but is not limited to this.

[0112] In some specific embodiments, the positive electrode material further includes a binder and / or a conductive agent.

[0113] The adhesive can be any conventional or commercially available adhesive material used for positive electrode sheets.

[0114] As an example, the adhesive includes, but is not limited to, one or more of polyvinyl alcohol, polyurethane, polyacrylate, polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, epoxy resin and chloroprene rubber.

[0115] The conductive agent can be any conventional or commercially available conductive material used for the positive electrode.

[0116] As an example, the conductive agent includes one or more of SP (conductive carbon black) and CNT (carbon nanotubes), but is not limited thereto.

[0117] Fourthly, the present invention provides a lithium-ion battery, including the positive electrode sheet as described above.

[0118] In some specific embodiments, the lithium-ion battery includes a casing, and a positive electrode, a negative electrode, a separator, and an electrolyte disposed within the casing, wherein the positive electrode includes the composite positive electrode material as described above.

[0119] The negative electrode sheet, separator, and electrolyte can be any commercially available negative electrode sheet, separator, and electrolyte, or any negative electrode sheet, separator, and electrolyte made using any existing technology. This invention does not limit the specific type of negative electrode sheet, separator, and electrolyte.

[0120] Lithium-ion batteries made using the composite cathode material provided by this invention have high capacity and excellent cycle stability.

[0121] The embodiments of the present invention will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be considered as limiting the scope of the invention. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer are followed. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0122] Example 1

[0123] The method for preparing the composite cathode material provided in this embodiment includes the following steps:

[0124] (1) Co3O4, Li2CO3 and Y2O3 were mixed in a high-speed mixer at a speed of 1200 r / min for 25 min. The molar ratio of lithium to cobalt was 1.05:1. The mass of Y2O3 accounted for 1000 ppm of the mass of Co3O4. The mixture was then subjected to two-stage calcination. Specifically, in the first stage, the mixture was heated to 500℃ at a heating rate of 5℃ / min and held at that temperature for 5 h. In the second stage, the mixture was heated to 1050℃ at a heating rate of 3℃ / min and held at that temperature for 8 h. After cooling, the mixture was crushed until the median particle size D50 of the lithium cobalt oxide powder was 17.8 μm. The lithium cobalt oxide material was obtained with a Y doping amount of 902 ppm.

[0125] (2) The ternary precursor Ni 0.8 Co 0.1 Mn 0.1 (OH)₂ was heated at 300℃ for 2 hours to obtain nickel-cobalt-manganese oxide. The nickel-cobalt-manganese oxide was then mixed with LiOH and SrO, with a molar ratio of Li to the total amount of nickel-cobalt-manganese transition metals of 1.02:1. The mass percentage of SrO was [missing information - likely a percentage of Ni]. 0.8 Co 0.1 Mn 0.1The Sr doping amount was 500 ppm (OH)2, and then sintered in air atmosphere. The temperature was increased from room temperature to 700℃ at a heating rate of 5℃ / min and sintered for 12h. After cooling to room temperature, the material was crushed to obtain a lithium nickel cobalt manganese oxide material with a median particle size D50 of 3.6μm. The Sr doping amount in the lithium nickel cobalt manganese oxide material was 485 ppm.

[0126] (3) Lithium sulfate, magnesium sulfate, ammonium phosphate and tartaric acid were added to deionized water in a molar ratio of 1:1.15:1.1:5. The lithium cobalt oxide material prepared in step (1) and the lithium nickel cobalt manganese oxide material prepared in step (2) were added to the above solution in a mass ratio of 7:2. The lithium cobalt oxide material and the lithium nickel cobalt manganese oxide material were added according to the mass of magnesium lithium phosphate being 0.5% of the total mass of the composite cathode material. The mixture was stirred for 7 hours in a water bath at 60°C to carry out a sol-gel reaction. The pH value of the mixture during the sol-gel reaction was 9.0. After the reaction was completed, a gel was obtained. The gel was dried at 100°C and sintered at 500°C for 2 hours and 800°C for 2 hours in sequence. After cooling, the mixture was sieved to obtain a composite cathode material with a median particle size D50 of 15.6 μm.

[0127] The composite cathode material prepared in this embodiment has a core-shell structure. The core of the core-shell structure includes lithium cobalt oxide and lithium nickel cobalt manganese oxide, and the outer shell of the core-shell structure includes lithium magnesium phosphate.

[0128] like Figure 1 The image shown is a SEM image of the composite cathode material prepared in this embodiment.

[0129] Example 2

[0130] The method for preparing the composite cathode material provided in this embodiment includes the following steps:

[0131] (1) Co3O4, LiOH and NbO were mixed in a high-speed mixer at a speed of 1100 r / min for 28 min. The molar ratio of lithium to cobalt was 1.08:1. The mass of NbO accounted for 1000 ppm of the mass of Co3O4. The mixture was then subjected to two-stage calcination. Specifically, in the first stage, the mixture was heated to 800℃ at a heating rate of 9℃ / min and held at that temperature for 4 h. In the second stage, the mixture was heated to 1000℃ at a heating rate of 2℃ / min and held at that temperature for 11 h. After cooling, the mixture was crushed until the median particle size D50 of the lithium cobalt oxide powder was 17.9 μm. The lithium cobalt oxide material was obtained with a Nb doping amount of 952 ppm.

[0132] (2) The ternary precursor Ni 0.8 Co 0.1 Al 0.1(OH)2 was heated at 350℃ for 1.5 h to obtain nickel cobalt aluminum oxide. The nickel cobalt aluminum oxide was mixed with Li2CO3 and WO3, with a molar ratio of Li to the total amount of nickel cobalt aluminum oxide of 1.05:1. The mass of WO3 accounted for 800 ppm of the mass of Co3O4. Then, it was sintered in an air atmosphere, heated from room temperature to 550℃ at a heating rate of 6℃ / min and sintered for 15 h. After cooling to room temperature, it was crushed to obtain lithium nickel cobalt aluminum oxide material with a median particle size D50 of 3.5 μm. The doping amount of W in the lithium nickel cobalt aluminum oxide material was 782 ppm.

[0133] (3) Lithium carbonate, magnesium nitrate, sodium phosphate and ammonium sulfate were added to deionized water in a molar ratio of 1:1:1:5. The lithium cobalt oxide material prepared in step (1) and the lithium nickel cobalt aluminum oxide material prepared in step (2) were added to the above solution in a mass ratio of 9:2. The lithium cobalt oxide material and the lithium nickel cobalt aluminum oxide material were added according to the calculation that the mass of lithium magnesium phosphate was 0.8% of the total mass of the composite cathode material. The mixture was stirred for 6.5 h in a water bath at 70 °C to carry out a sol-gel reaction. The pH value of the mixture during the sol-gel reaction was 8.5. After the reaction was completed, a gel of lithium magnesium phosphate coated core matrix (including lithium cobalt oxide material and ternary material) was obtained. The gel was dried at 110 °C and sintered at 450 °C for 2.5 h and 800 °C for 2 h in sequence. After cooling, it was sieved to obtain a composite cathode material with a median particle size D50 of 14.9 μm.

[0134] The composite cathode material prepared in this embodiment has a core-shell structure. The core of the core-shell structure includes lithium cobalt oxide material and lithium nickel cobalt aluminum oxide material, and the outer shell material includes lithium magnesium phosphate.

[0135] Example 3

[0136] The method for preparing the composite cathode material provided in this embodiment includes the following steps:

[0137] (1) Co(OH)2, LiNO3, MgO and Al2O3 were mixed in a high-speed mixer at 1100 r / min for 28 min, wherein the molar ratio of lithium to cobalt was 1.08:1, and the mass of MgO and Al2O3 accounted for 8000 ppm of the mass of Co3O4. The mixture was then subjected to two-stage calcination. Specifically, in the first stage, the mixture was heated to 500℃ at a heating rate of 3℃ / min and held at that temperature for 7 h. In the second stage, the mixture was heated to 1100℃ at a heating rate of 4℃ / min and held at that temperature for 6 h. After cooling, the mixture was crushed to a median particle size D50 of 18.6 μm to obtain lithium cobalt oxide material. The doping amount of Mg in the lithium cobalt oxide material was 976 ppm and the doping amount of Al was 6912 ppm.

[0138] (2) The ternary precursor Ni 0.6 Co 0.2 Mn 0.2 (OH)2 was heated at 300℃ for 2 h to obtain nickel cobalt manganese oxide. The nickel cobalt manganese oxide was mixed with Li2CO3 and ZrO2, wherein the molar ratio of Li to the total amount of nickel cobalt manganese was 1.06:1, and the mass of ZrO2 accounted for 1000 ppm of the mass of Co3O4. Then, it was sintered in an air atmosphere, and the temperature was increased from room temperature to 800℃ at a heating rate of 5℃ / min and sintered for 10 h. After cooling to room temperature, it was crushed to obtain lithium nickel cobalt manganese oxide material with a median particle size D50 of 4.1 μm and a Zr doping amount of 947 ppm in the lithium nickel cobalt manganese oxide material.

[0139] (3) Lithium acetate, magnesium sulfate, potassium phosphate, and tartaric acid were added to deionized water in a molar ratio of 1:0.95:1.1:5. The lithium cobalt oxide material prepared in step (1) and the lithium nickel cobalt manganese oxide material prepared in step (2) were added to the above solution in a mass ratio of 6:2. The lithium cobalt oxide material and the lithium nickel cobalt manganese oxide material were added according to the mass of lithium magnesium phosphate being 1.0% of the total mass of the composite cathode material. The mixture was stirred for 6.5 h in a water bath at 75°C to carry out a sol-gel reaction. The pH value of the mixture during the sol-gel reaction was 9.5. After the reaction was completed, a gel of lithium magnesium phosphate coated core matrix (including lithium cobalt oxide material and ternary material) was obtained. The gel was dried at 120°C and then sintered at 550°C for 2 h and 800°C for 2 h respectively. After cooling, the mixture was sieved to obtain a composite cathode material with a median particle size D50 of 15.2 μm.

[0140] The composite cathode material prepared in this embodiment has a core-shell structure. The core of the core-shell structure includes lithium cobalt oxide and lithium nickel cobalt manganese oxide, and the outer shell of the core-shell structure includes lithium magnesium phosphate.

[0141] Example 4

[0142] The preparation method of the composite cathode material provided in this embodiment is basically the same as that in Example 1. The difference is that in step (1), Y2O3 is replaced with an equimolar amount of Ga2O3.

[0143] Example 5

[0144] The preparation method of the composite cathode material provided in this embodiment is basically the same as that in Example 1. The difference is that in step (1), Y2O3 is replaced with an equimolar amount of In2O3.

[0145] Example 6

[0146] The preparation method of the composite cathode material provided in this embodiment is basically the same as that in Example 1. The difference is that in step (1), Y2O3 is replaced with an equimolar amount of V2O5.

[0147] Example 7

[0148] The preparation method of the composite cathode material provided in this embodiment is basically the same as that in Example 1. The difference is that in step (2), SrO is replaced with an equimolar amount of CaO.

[0149] Example 8

[0150] The preparation method of the composite cathode material provided in this embodiment is basically the same as that in Example 1. The difference is that in step (2), SrO is replaced with an equimolar amount of TiO2.

[0151] Example 9

[0152] The preparation method of the composite cathode material provided in this embodiment is basically the same as that in Example 1, except that the Ni in step (2) is... 0.8 Co 0.1 Mn 0.1 (OH)₂ is replaced with an equimolar amount of a mixed precursor material, wherein the mixed precursor material is Ni in a mass ratio of 1:1. 0.8 Co 0.1 Mn 0.1 (OH)2 and Ni 0.8 Co 0.1 Al 0.1 (OH)2.

[0153] Example 10

[0154] The preparation method of the composite cathode material provided in this embodiment is basically the same as that in Example 1. The difference is that in step (1), the two-stage calcination is replaced by a single calcination, specifically: heating to 1050°C at a heating rate of 4°C / min and holding for 13 hours.

[0155] Example 11

[0156] The preparation method of the composite cathode material provided in this embodiment is basically the same as that in Example 1, except that the Ni in step (2) is... 0.8 Co 0.1 Mn 0.1 (OH)2 is replaced with Ni 0.5 Co 0.2 Mn 0.3 (OH)2.

[0157] Example 12

[0158] The preparation method of the composite cathode material provided in this embodiment is basically the same as that in Example 1. The difference is that the mass ratio of lithium cobalt oxide material and ternary material in step (3) is 6:5.

[0159] Comparative Example 1

[0160] The method for preparing the composite cathode material provided in this comparative example includes the following steps:

[0161] (1) Same as step (1) in Example 1.

[0162] (2) Same as step (2) in Example 1.

[0163] (3) The lithium cobalt oxide material obtained in step (1) with a mass ratio of 3.5:1 and the ternary material obtained in step (2) are mixed and sintered at 500°C for 5 hours. After cooling, the mixture is sieved to obtain the composite cathode material.

[0164] That is, the composite cathode material prepared in this comparative example does not have a lithium magnesium phosphate shell.

[0165] Comparative Example 2

[0166] The method for preparing the composite cathode material provided in this comparative example includes the following steps:

[0167] (1) Following the same steps as in Example 1, lithium cobalt oxide powder was obtained.

[0168] (2) Co3O4, LiOH and SrO were mixed, with the molar ratio of Li element to ternary precursor and Sr element being the same as in Example 1. The mixture was sintered in an air atmosphere, heated from room temperature to 700℃ at a heating rate of 5℃ / min for 12h, and then cooled to room temperature and crushed to obtain small lithium cobalt oxide powder with an average particle size of 3.6μm.

[0169] (3) is basically the same as step (3) in Example 1, except that the ternary material is replaced with the lithium cobalt oxide powder obtained in step (2) of this comparative example.

[0170] That is, the core of the composite cathode material prepared in this comparative example does not contain lithium nickel cobalt manganese oxide material.

[0171] Comparative Example 3

[0172] The preparation method of the composite cathode material provided in this comparative example is basically the same as that in Example 1, except that in step (3), the lithium cobalt oxide material is replaced with an equal mass of ternary material.

[0173] That is, the core of the composite cathode material prepared in this comparative example does not contain lithium cobalt oxide material.

[0174] Comparative Example 4

[0175] The preparation method of the composite cathode material provided in this comparative example is basically the same as that in Example 1. The difference is that in step (3), magnesium sulfate is replaced with an equal amount of ferrous sulfate, and lithium cobalt oxide material and ternary material are added according to the mass of lithium iron phosphate being 0.5% of the total mass of the composite cathode material.

[0176] That is, the outer shell of the composite cathode material prepared in this comparative example is lithium iron phosphate.

[0177] Comparative Example 5

[0178] The preparation method of the composite cathode material provided in this comparative example is basically the same as that in Example 1. The difference is that in step (3), magnesium sulfate is replaced with an equal amount of zirconium sulfate, and lithium cobalt oxide material and ternary material are added according to the mass of lithium zirconium phosphate being 0.5% of the total mass of the composite cathode material.

[0179] That is, the outer shell of the composite cathode material prepared in this comparative example is lithium zirconium phosphate.

[0180] The median particle size D50 mentioned above was measured using the test method in GB / T19077.1.

[0181] Experimental Example 1

[0182] The tap density, compaction density, and specific surface area of ​​the composite cathode materials prepared in each embodiment and comparative example were tested using a tap density tester, a compaction density tester, and a specific surface area tester, respectively. The results are shown in Table 1.

[0183] Among them, tap density: the test method in GB / T5162 is adopted;

[0184] Compacted density: Tested using a compacted density tester under a pressure of 150 MPa;

[0185] Specific surface area: The test method in GB / T13390 shall be adopted.

[0186] Table 1. Test results of tapped density, compacted density, and specific surface area:

[0187] Group <![CDATA[Tap density (g / cm 3 )]]> <![CDATA[Compaction density (g / cm 3 )]]> <![CDATA[Specific surface area (m 2 / g)]]> Example 1 2.87 3.87 0.22 Example 2 2.92 3.83 0.21 Example 3 3.02 3.84 0.20 Example 4 2.88 3.94 0.21 Example 5 2.93 3.89 0.21 Example 6 2.89 3.91 0.22 Example 7 2.86 3.94 0.19 Example 8 2.96 3.95 0.23 Example 9 3.01 3.89 0.24 Example 10 2.81 3.83 0.19 Example 11 2.80 3.82 0.22 Example 12 2.81 3.80 0.17 Comparative Example 1 2.48 3.75 0.14 Comparative Example 2 2.71 3.70 0.18 Comparative Example 3 2.73 3.74 0.17 Comparative Example 4 2.81 3.75 0.18 Comparative Example 5 2.80 3.78 0.16

[0188] Experimental Example 2

[0189] The composite positive electrode materials prepared in each embodiment and comparative example were used as the positive electrode active material. Acetylene black was used as the conductive agent, and polyvinylidene fluoride was used as the binder. The mass ratio of the three was 90:5:5. N-methylpyrrolidone was added, and the mixture was stirred evenly to form a slurry. This slurry was then coated onto an aluminum foil current collector, vacuum dried, pressed into sheets, and cut into positive electrode sheets of the required size. The coin-type lithium-ion battery was assembled from the above-mentioned positive electrode sheet, lithium negative electrode, separator between the positive and negative electrodes, and electrolyte. The assembled battery was used for capacity testing and cycle testing. The test results are shown in Table 2.

[0190] The cycle performance test method is as follows: under 45℃ conditions, the button cell is charged at 0.1C and discharged at 0.1C for 50 cycles, with a voltage range of 3V to 4.6V.

[0191] Table 2. Capacity and Cyclic Performance Test Results:

[0192]

[0193] As shown in Table 2, the composite cathode materials prepared in each embodiment have high capacity and cycle life when used as batteries.

[0194] Compared to Example 1, Example 10 resulted in a decrease in capacity and cycle life because the lithium cobalt oxide material was not prepared using a two-stage calcination process.

[0195] Compared to Example 1, Example 11 uses a different type of precursor, resulting in a decrease in capacity and cycle life.

[0196] Compared to Example 1, Example 12 has a higher proportion of large-particle lithium cobalt oxide material, resulting in lower tap density, compaction density, and specific surface area.

[0197] Compared to Example 1, Comparative Example 1, due to the absence of a lithium magnesium phosphate casing, resulted in a decrease in both the initial discharge specific capacity and cycle life of the lithium-ion battery.

[0198] Compared to Example 1, Comparative Example 2 has a lower cycle life for lithium-ion batteries because it does not contain lithium nickel cobalt manganese oxide materials in its core, and this also results in a higher cost for the cathode material.

[0199] Compared to Example 1, Comparative Example 3 has a lower initial discharge specific capacity of lithium-ion batteries because it does not contain lithium cobalt oxide material in its core.

[0200] Compared to Example 1, Comparative Examples 4 and 5 have lower initial discharge specific capacity and cycle life of lithium-ion batteries due to the use of different casing materials.

[0201] In summary, the present invention provides a composite cathode material with a core-shell structure consisting of lithium cobalt oxide and ternary materials as the core and lithium magnesium phosphate as the shell. The battery made from this material exhibits high capacity and cycle performance at high voltage.

[0202] Furthermore, by adjusting the types of doping elements in lithium cobalt oxide and ternary materials, the composition of the precursor, the sintering method, and parameters such as the specific surface area, tap density, and compaction density of the composite cathode material, this invention can further improve the capacity or cycle performance of lithium-ion batteries containing composite cathode materials.

[0203] Although the present invention has been illustrated and described with specific embodiments, it should be understood that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; those skilled in the art should understand that modifications can be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein, without departing from the spirit and scope of the present invention; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention; therefore, this means that all such substitutions and modifications that fall within the scope of the present invention are included in the appended claims.

Claims

1. A composite cathode material, characterized in that, The composite cathode material has a core-shell structure, wherein the core of the core-shell structure includes lithium cobalt oxide material and ternary material; wherein the ternary material includes lithium nickel cobalt manganese oxide material and / or lithium nickel cobalt aluminum oxide material; The outer shell of the core-shell structure comprises lithium magnesium phosphate; the mass of the lithium magnesium phosphate is 0.01% to 5% of the total mass of the composite cathode material; The lithium cobalt oxide material includes lithium cobalt oxide and E element doped in the lithium cobalt oxide, wherein E includes at least one of Ca, Sr, Ga, Ge, In, Al, Sc, Ti, V, Cr, Mn, Fe, Ni, Cu, Y, Zr, Nb, Mo, Ru, Rh, Pd, Ag, La, Hf, Ta, W, Re, Os, Ir, Pt and Au; The lithium nickel cobalt manganese oxide material includes lithium nickel cobalt manganese oxide and element A doped in the lithium nickel cobalt manganese oxide, wherein A includes at least one of Ca, Sr, Ga, Ge, In, Al, Sc, Ti, V, Cr, Fe, Cu, Y, Zr, Nb, Mo, Ru, Rh, Pd, Ag, La, Hf, Ta, W, Re, Os, Ir, Pt and Au; The lithium nickel cobalt aluminum oxide material includes lithium nickel cobalt aluminum oxide and Q element doped in the lithium nickel cobalt aluminum oxide, wherein Q includes at least one of Ca, Sr, Ga, Ge, In, Sc, Ti, V, Cr, Fe, Cu, Y, Zr, Nb, Mo, Ru, Rh, Pd, Ag, La, Hf, Ta, W, Re, Os, Ir, Pt and Au; The capacity retention rate of lithium-ion batteries containing the aforementioned composite cathode material is 85.4%~92.2% after 50 cycles at 45°C. The preparation method of the composite cathode material includes the following steps: mixing lithium cobalt oxide material, ternary material, phosphorus source, magnesium source, lithium source, dispersant and solvent and carrying out sol-gel reaction to obtain gel; subjecting the gel to first sintering and second sintering, and cooling to obtain the composite cathode material; the median particle size D50 of the lithium cobalt oxide material is 14~20μm; the median particle size D50 of the ternary material is 3~8μm; the mass ratio of the lithium cobalt oxide material to the ternary material is 6~10:2~5.

2. The composite cathode material according to claim 1, characterized in that, It contains at least one of the following features (1) to (3): (1) The E element doping amount in the lithium cobalt oxide material is 100~20000ppm; (2) The doping amount of element A in the lithium nickel cobalt manganese oxide material is 100~9000ppm; (3) The doping amount of Q element in the lithium nickel cobalt aluminum oxide material is 100~9000ppm.

3. The composite cathode material according to claim 1, characterized in that, It contains at least one of the following features (1) to (4): (1) The specific surface area of ​​the composite cathode material is 0.17~0.24 m². 2 / g; (2) The tap density of the composite cathode material is 2.8~3.2 g / cm³. 3 ; (3) The compaction density of the composite cathode material is 3.8~4.3 g / cm³. 3 ; (4) The median particle size D50 of the composite cathode material is 13~17μm.

4. The composite cathode material according to claim 1, characterized in that, The lithium-ion battery containing the composite cathode material has a first charge specific capacity of 216~225mAh / g at 0.1C; And / or, the lithium-ion battery containing the composite cathode material has an initial discharge specific capacity of 194.5~206 mAh / g at 0.1C; And / or, the lithium-ion battery containing the composite cathode material has an initial coulombic efficiency of 89.8% to 93.0% at 0.1C.

5. The method for preparing the composite cathode material according to any one of claims 1 to 4, characterized in that, Includes the following steps: Lithium cobalt oxide material, ternary material, phosphorus source, magnesium source, lithium source, dispersant and solvent are mixed and subjected to sol-gel reaction to obtain gel; The gel is subjected to a first sintering and a second sintering, and then cooled to obtain the composite cathode material. The median particle size D50 of the lithium cobalt oxide material is 14~20μm; The median particle size D50 of the ternary material is 3~8μm; The mass ratio of the lithium cobalt oxide material to the ternary material is 6~10:2~5.

6. The method for preparing the composite cathode material according to claim 5, characterized in that, It contains at least one of the following features (1) to (7): (1) During the sol-gel reaction, the temperature of the mixture is 60~80℃; (2) During the sol-gel reaction, the pH value of the mixture is 8~10; (3) The sol-gel reaction time is 6~8h; (4) The temperature of the first sintering is 400~600℃; (5) The second sintering temperature is 700~900℃; (6) The ternary material includes lithium nickel cobalt manganese oxide material and lithium nickel cobalt aluminum oxide material with a mass ratio of 1~5:0~1; (7) The dispersant includes at least one of ammonia, ammonium chloride, ammonium sulfate, ammonium carbonate, citric acid and tartaric acid.

7. The method for preparing the composite cathode material according to claim 5, characterized in that, The lithium cobalt oxide material is mainly prepared by mixing a lithium source, a cobalt source, and an E-containing compound and then calcining them in two stages.

8. The method for preparing the composite cathode material according to claim 7, characterized in that, The two-stage calcination specifically includes: first holding at 400~900℃ for 3~8 hours, and then holding at 950~1200℃ for 5~12 hours.

9. A positive electrode sheet, characterized in that, Includes the composite cathode material as described in any one of claims 1 to 4.

10. A lithium-ion battery, characterized in that, Including the positive electrode sheet as described in claim 9.

Citation Information

Patent Citations

  • High-voltage composite positive electrode material and lithium ion battery containing same

    CN112563462A

  • Lithium cobalt oxide positive electrode material and preparation method thereof, positive electrode plate, secondary battery and electric device

    CN116995207A