Porous carbon material, carbon-coated metal composite porous carbon material, preparation method thereof, negative electrode sheet and lithium ion battery
Porous carbon materials were prepared by etching and spray freeze-drying, and then carbon-coated metal was deposited on their surface. This method solved the shortcomings of graphite-based anode materials in terms of capacity and cycle performance, improved the overall performance of lithium-ion batteries, and is suitable for various types of lithium-ion batteries.
Patent Information
- Application Number
- CN202311418085.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-10-30
AI Technical Summary
Existing graphite-based anode materials have limited lithium capacity and struggle to achieve both high rate capability and long cycle life. Modification treatments are not very effective and cannot meet the comprehensive performance requirements of power batteries.
Porous carbon materials were prepared by etching graphite materials in an alkaline solution using a non-metallic catalyst, and nanoscale lithium metal particles were deposited by spray freeze-drying. Subsequently, carbon was coated on the surface of the porous carbon materials by vapor deposition to form a carbon-coated metal composite porous carbon material.
It achieves uniform pore size distribution in porous carbon materials and uniform lithium metal distribution, improving the lithium insertion and delithiation capacity efficiency of lithium-ion batteries, enhancing the battery's electrical and safety performance, and is suitable for conventional lithium-ion batteries and gel polymer membrane lithium batteries.
Smart Images

Figure CN117525374B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion batteries, specifically relating to a porous carbon material, a carbon-coated metal composite porous carbon material, its preparation method, a negative electrode sheet, and a lithium-ion battery. Background Technology
[0002] Currently, lithium-ion batteries are widely used in power and energy storage fields. Conventional lithium-ion batteries include a positive electrode, a negative electrode, a carrier for ion conduction in the battery, and a separator that isolates the active materials of the positive and negative electrodes and ensures the ion channels. The negative electrodes used in lithium-ion batteries are mainly carbon negative electrodes and non-carbon negative electrodes. Carbon materials include graphite-based negative electrode materials, intermediate carbon microspheres, graphene, hard carbon, and soft carbon. Non-carbon materials include silicon-based negative electrode materials, lithium titanate negative electrode materials, and other non-carbon materials. Currently, carbon materials are widely used, especially graphite materials, which are mature in application. However, the layered structure of graphite has a limited capacity for lithium and cannot simultaneously achieve high rate and long cycle performance, so it is necessary to modify the current graphite materials.
[0003] There are many types of production processes for graphite anode materials. However, the current morphology and properties of graphite are not suitable for the various forms of lithium-ion batteries. Graphite needs to be modified. Current reports on graphite modification generally focus on graphite composites with silicon-based anodes, different types of carbon coatings on graphite, and metal element coating processes. These methods can only address one aspect of the material's capacity or performance, and do not significantly improve the overall performance, thus limiting its application range. Therefore, it is necessary to improve the capacity of graphite materials while simultaneously enhancing their cycle and rate performance for application in different lithium-ion batteries, breaking through material barriers, and meeting the demands of the power battery market. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a porous carbon material, a carbon-coated metal composite porous carbon material, its preparation method, a negative electrode sheet and a lithium-ion battery.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0006] A porous carbon material containing etched pores; the pore size of the etched pores is 100 nm-4 μm, and the pore volume is 1.39-1.57 cm³. 3 / g.
[0007] Preferably, the hole is a round hole.
[0008] The present invention also includes a method for preparing a porous carbon material, comprising the following steps: graphite material is prepared by etching in an alkaline solution using a non-metallic catalyst.
[0009] The alkaline solution is an aqueous solution of one or at least two of LiOH, Zn(OH)2, and Ca(OH)2.
[0010] The non-metallic catalyst is one or a mixture of at least two of phosphorene, black phosphorus, lithium sulfide, boron nitride, boron phosphate, lithium phosphide, and magnesium silicate; preferably, the mass ratio of the non-metallic catalyst to the graphite material is 1%-10%. The addition of a high content of non-metallic catalyst will coat the surface of the active graphite material. Excessive loading leads to excessively large pore sizes in the etched material, with less connection between pore walls, resulting in large, interconnected pores and damaging the material's structure. This is detrimental to the subsequent processing performance and lithium ion insertion / extraction. Therefore, it is necessary to control the mass ratio of the non-metallic catalyst to be less than or equal to 10% of the graphite material mass.
[0011] The preparation method of porous carbon material specifically includes the following steps: 1) adding graphite material to an alkaline solution containing a non-metallic catalyst, stirring evenly and then drying; 2) calcining the dried material obtained in step 1); 3) washing and drying with an acidic solution after calcination to obtain porous carbon material.
[0012] The calcination temperature in step 2) is 350-700℃, preferably 1-3h, and most preferably 2h. After calcination, the porous graphite material has a uniform pore size distribution, consisting of 100nm-4μm round pores. As the etching and calcination time increases, the pore distribution and pore size will increase. By adjusting the calcination time, the pore size and depth can be gradually increased. The charge-discharge curves of coin cells assembled from porous carbon materials obtained with different calcination (etching) times show that the material calcined (etched) for 2 hours has the best charge-discharge capacity.
[0013] The graphite material is a composite of primary and / or secondary particles; its particle size D50 is ≥8μm, the graphite particles are uniform in size, and the degree of graphitization is ≥95%.
[0014] The present invention also includes a carbon-coated metal composite porous carbon material, comprising a metal composite porous carbon material and carbon coated thereon, wherein the metal composite porous material comprises the porous carbon material and lithium metal disposed in the pores of the porous carbon material;
[0015] Preferably, the lithium metal accounts for 5%-50% of the pore volume in the metal composite porous carbon material, and more preferably 30%.
[0016] Preferably, the carbon coating amount of the carbon-coated metal composite porous carbon material accounts for 0.5%-3% of the mass of the metal composite porous carbon material, with a preferred ratio of 1.2%.
[0017] This invention also includes a method for preparing the aforementioned carbon-coated metal composite porous carbon material, comprising the following steps:
[0018] 1) Lithium metal is heated to the point of melting in an inert gas and then freeze-dried by spray to produce hollow lithium metal spheres of 100nm-50μm. The lithium metal is melted and then freeze-dried by spray, taking advantage of the principle that the molten lithium metal becomes hard and brittle after instantaneous cooling. The nano- and submicron-sized lithium metal particles are produced by using a spray freeze dryer, resulting in hollow lithium metal spheres of 100nm-50μm.
[0019] 2) The porous carbon material and the lithium metal hollow spheres obtained in step 1) are mixed in an inert gas and heated to 200-450°C and kept at that temperature for 4-8 hours, preferably heated to 400°C and kept at that temperature for 8 hours, and then cooled to room temperature to obtain a metal composite porous carbon material.
[0020] Preferably, the proportion of lithium metal hollow spheres in the porous carbon material is 7%-44%, and more preferably 20%; preferably, lithium metal occupies 5%-50% of the pores in the metal composite porous carbon material, and more preferably 30%.
[0021] 3) The obtained metal composite porous carbon material is subjected to carbon source gas vapor deposition to obtain carbon-coated metal composite porous carbon material. The temperature of carbon deposited on the surface of the metal composite porous carbon is controlled to be below 150℃.
[0022] Preferably, the carbon source gas is methane or ethane;
[0023] Preferably, the carbon coating amount of the carbon-coated metal composite porous carbon material accounts for 0.5%-3% of the mass ratio of the composite material, with a preferred ratio of 1.2%.
[0024] The carbon-coated metal composite porous carbon material was used to make a button cell CO2032 material. The material has a lithium intercalation capacity of 1640.98 mAh / g and a lithium deintercalation capacity of 1587.3 mAh / g, with an efficiency of over 96.7%. Lithium metal has a huge advantage in capacity efficiency. The capacity can be adjusted by adjusting the amount of lithium metal deposited. Lithium metal can reach 50% of the pore size and the capacity can reach over 2500 mAh / g.
[0025] The present invention also includes a negative electrode sheet comprising the aforementioned porous carbon material or the aforementioned carbon-coated metal composite porous carbon material.
[0026] The present invention also includes a lithium-ion battery, comprising the aforementioned negative electrode sheet; preferably, the lithium-ion battery is a gel polymer membrane battery and a gel electrode battery.
[0027] Compared with the prior art, the beneficial effects of the present invention are:
[0028] The porous carbon material of this invention is mainly aimed at the modification of graphite anodes. It uses a non-metallic catalyst to directionally etch graphite material, resulting in porous carbon material with controllable pore size and uniform distribution.
[0029] The lithium metal solution is freeze-dried at low temperature to form nano- or micro-sized spherical hollow lithium metal particles, which are then deposited onto the surface of porous carbon materials. The lithium metal is evenly distributed and is easy to industrialize.
[0030] Based on this, carbon coating by vapor deposition was carried out on the surface of porous carbon materials with deposited lithium metal to enhance their electrical and safety performance, fill the technical gap of lithium metal deposition through etched holes, and can be applied to conventional lithium-ion batteries, gel polymer membrane lithium batteries and gel electrode lithium batteries. Attached Figure Description
[0031] Figure 1 In the example, a and b are SEM images of graphite particles in samples A and B without any treatment, respectively.
[0032] Figure 2 SEM images of graphite etched at different times in the examples;
[0033] Figure 3 The figures show the charge-discharge curves after etching at different times in the examples;
[0034] Figure 4 The figure shows the pore volume and pore size distribution curves of graphite before and after etching in the embodiment.
[0035] Figure 5 This is a comparison image of EIS after 2 hours of etching and without etching in the example;
[0036] Figure 6 A comparison of the charge-discharge performance of a coin cell made of graphite before and after etching, as shown in the example.
[0037] Figure 7 A comparison of the cycle performance of coin cells made of graphite before and after etching, as shown in the example.
[0038] Figure 8 This is a SEM image of the porous carbon material after etching in Comparative Example 1 without the addition of a non-metallic catalyst.
[0039] Figure 9 SEM image of the carbon-coated metal composite carbon material in the example;
[0040] Figure 10 EDS analysis diagram of carbon-coated metal composite material in the example;
[0041] Figure 11 Schematic diagram of a gel polymer membrane lithium battery and a gel-state electrode battery fabricated for an example;
[0042] Figure 12 The charge-discharge curves of a button battery made of carbon-coated metal composite carbon material are shown in the example. Detailed Implementation
[0043] To enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings and preferred embodiments.
[0044] Example 1
[0045] A method for preparing porous carbon materials, wherein the graphite material is prepared by etching in an alkaline solution using a non-metallic catalyst.
[0046] Specifically, the steps are as follows: 1) First, add 2 mol of Ca(OH)2 (which can be replaced with LiOH or Zn(OH)2, with Ca(OH)2 being preferred) to 1000 ml of water to prepare a 2 mol / L alkaline solution of Zn(OH)2. Sample A consists of secondary graphite particles with a particle size D50 of 12 μm, and sample B consists of primary graphite particles with a particle size D50 of 11 μm. Add 5 g of the non-metallic catalyst boron nitride, and then add sample A ( Figure 1 (as shown in a) or sample B ( Figure 1 (As shown in b) 500g of sample was added to a Ca(OH)2 solution and stirred with a mechanical stirrer for 30-60 minutes to make a muddy solution. Then it was dried in a forced-air oven at 100℃ for 8 hours.
[0047] 2) Calcine the dried material obtained in step 1) at 650°C (which can be adjusted to 350°C, 500°C and 700°C, with 650°C being the best result, and therefore is used as an example) for 1 hour in an inert atmosphere.
[0048] 3) After calcination, the material was washed with 1 mol / L hydrochloric acid until neutral, and then dried to obtain porous carbon material.
[0049] Example 2
[0050] The difference between Example 2 and Example 1 is that in step 2), calcination is performed for 2 hours.
[0051] Example 3
[0052] The difference between Example 3 and Example 1 is that in step 2), calcination is carried out for 3 hours.
[0053] Figure 2 The image shows electron microscope (EM) images of porous carbon materials obtained after calcining (etching) graphite material sample A for 1 hour (Example 1), 2 hours (Example 2), and 3 hours (Example 3). Figure 2In the image, a (untreated graphite) is graphite material sample A; b1 and b2 are electron microscope images of porous carbon material at different magnifications after calcination (etching) for 1 hour; c1 and c2 are electron microscope images of porous carbon material at different magnifications after calcination (etching) for 2 hours; and d1 and d2 are electron microscope images of porous carbon material at different magnifications after calcination (etching) for 3 hours.
[0054] The results showed that the pore size distribution after calcination for 1-3 hours was uniform, with 100 nm-4 μm round pores. As the etching and calcination time increased, the pore distribution and pore size increased. By adjusting the calcination time, the pore size and depth could be gradually increased. The porous carbon materials after calcination (etching) at different times were used to make negative electrode sheets and then made into button cells C02032.
[0055] Figure 3 The charge-discharge curves of coin cells assembled from porous carbon materials obtained by different calcination (etching) times are shown. Comparing the 0.2C charge-discharge curves of different etching times, it can be seen that the discharge specific capacity (lithium insertion capacity) of the porous carbon materials is 347.41 mAh / g, 366.87 mAh / g, 381.77 mAh / g, and 375.49 mAh / g for unetched (sample A graphite material), etched for 1 hour (Example 1), etched for 2 hours (Example 2), and etched for 3 hours (Example 3), respectively. The corresponding charging specific capacity (lithium removal capacity) of the porous carbon materials is 336.10 mAh / g, 343.85 mAh / g, 380.44 mAh / g, and 364 mAh / g.
[0056] After comparison, it was found that the material calcined (etched) for 2 hours had the best charge-discharge capacity. The material etched for 2 hours (Example 2) was selected for further modification.
[0057] Figure 4 The etching process lasted 2 hours, comparing the pore volume and pore size distribution of Example 2 (graphite after etching) and Sample A (graphite before etching). The pore volume after etching was 1.57 cm³. 3 / g, the hole volume before etching was 1.38cm³. 3 / g;
[0058] The porous carbon material obtained in Example 2 was used to fabricate a coin cell (CO2032). Graphite material sample A (unetched graphite) was used as a comparative example to prepare the electrode. A lithium-ion sheet was used as the positive electrode. After fabricating the coin cell, performance testing was performed. Figure 5 As shown, the coin cell made of porous carbon material (graphite after 2 hours of etching) exhibited a significant decrease in internal resistance in EIS testing; for example... Figure 6As shown, comparing the graphite material sample A (graphite before etching) and the porous carbon material after etching for 2 hours (graphite after etching), the porous carbon material in Example 2 can achieve a capacity of 356 mAh / g and a coulombic efficiency of 99.8% at a charge / discharge rate of 5C, while the graphite material sample A only has a capacity of 301 mAh / g and a coulombic efficiency of only 83%. The cycle performance of the coin cells was compared. Figure 7 The porous carbon material was subjected to room temperature cycling at 1C current for 300 cycles. After 2 hours of etching, the porous carbon material (after etching in the figure) showed almost no capacity decay. After 300 cycles, the capacity retention of the etched porous carbon material was 89.5%.
[0059] Example 4
[0060] The difference between Example 4 and Example 2 is that the amount of boron nitride added was increased from 5g (1% of the graphite material by mass) to 10g (2%); other factors remained the same. The pore size and pore depth of the resulting porous carbon material increased by 1.5 times and 1.2 times compared to Example 2, indicating that the amount of non-metallic catalyst can control and adjust the pore depth and pore size.
[0061] Example 5
[0062] The difference between Example 5 and Example 2 is that the amount of boron nitride added is increased from 5g (1%) to 20g (4%), 30g (6%), 40g (8%), 50g (10%), and 60g (12%); all other amounts remain the same.
[0063] Table 1 shows the effect of different catalyst addition ratios on the pore volume and pore size after etching.
[0064]
[0065] As shown in Table 1, when 60g of catalyst was added, excessively large pores were formed on the surface, with the largest pore size reaching 7μm, which is close to the particle size of graphite itself. The addition of high boron nitride content will cover the surface of active graphite, resulting in excessive loading and causing the pore size of the etching material to be too large. There is less connection between the pore walls, and the pores are connected in series, forming large voids. The structure of the material is damaged, which is not conducive to the subsequent processing performance of the material and the deintercalation and deintercalation of lithium ions. Therefore, it is necessary to control the mass ratio of boron nitride catalyst to be less than or equal to 10% of the graphite mass.
[0066] Meanwhile, in this application, the non-metallic catalyst can be replaced with phosphorene, black phosphorus, lithium sulfide, boron nitride, boron phosphate, lithium phosphide, or magnesium silicate. By adjusting the amount used and the calcination conditions, pores with uniform pore size distribution and a diameter of 100 nm to 4 μm can be obtained. The total volume of the etched pores accounts for 5-70% of the volume of the porous carbon material. Boron nitride is used as a preferred example in this application for illustrative purposes.
[0067] Example 6
[0068] The preparation of a carbon-coated metal composite porous carbon material involves depositing lithium on the surface of the porous carbon material obtained in Example 2 to obtain the metal composite porous carbon material; specifically, it includes the following steps:
[0069] 1) 100g of lithium metal sheet was heated in an inert atmosphere to a temperature of 230℃. The lithium metal melted and was then freeze-dried using a spray freeze dryer. The principle is that the molten lithium metal becomes hard and brittle after instantaneous cooling. The process produced nano- and submicron-sized lithium metal particles, resulting in hollow lithium metal spheres with a diameter of 100nm-50μm.
[0070] 2) 100g of porous graphite material prepared in Example 2 is mixed with 20g of prepared lithium metal hollow spheres (which can be adjusted to 7g, 10g, 30g, or 44g, with 20g being the most effective). The mixture is placed in a dry atmosphere and in an inert Ar atmosphere at a temperature controlled at 400℃ (which can be adjusted to 200℃, 300℃, or 450℃, with 400℃ being the most effective, as illustrated in the example). The temperature is maintained for 8 hours (which can also be 4 hours or 6 hours, with 8 hours being the most effective). The mixture is then cooled to room temperature, and the lithium metal spheres are completely deposited in the pores, occupying 30% of the pores (adjusting the amount of different lithium metal hollow spheres can result in lithium metal occupying 5%-50% of the pores in the metal composite porous carbon material). The material is then vapor-deposited using methane or ethane, with the temperature of the porous carbon deposited by lithium metal controlled at 140℃, to obtain a coated metal composite carbon material with a carbon content of 1.2% (the carbon coating amount can be adjusted to 0.5% or 3%).
[0071] like Figure 9 As shown, the obtained carbon-coated metal composite carbon material has surface pores that are almost completely filled, and the surface is mainly composed of amorphous carbon; such as Figure 10 The EDS results from the tests in Table 2 showed that lithium metal accounted for 22.35% by mass and carbon accounted for 77.65% by mass. Converted to molar proportions, lithium metal accounted for 33% and carbon accounted for 67%.
[0072] Table 2 Figure 10 Analysis and comparison table
[0073]
[0074] The carbon-coated metal composite porous carbon material was used to make a button cell CO2O32 material with a lithium content of 22%. Figure 12The material has a lithium insertion capacity of 1640.98 mAh / g and a delithiation capacity of 1587.3 mAh / g, with an efficiency of over 96.7%. Lithium metal has a significant advantage in capacity efficiency. The capacity can be adjusted by changing the amount of lithium metal deposited. Lithium metal can account for 50% of the pore size, and the capacity can reach over 2500 mAh / g.
[0075] Example 7
[0076] The preparation of a lithium-ion battery includes the following steps:
[0077] 1) Preparation of negative electrode sheet: The carbon-coated metal composite porous carbon material obtained in Example 6 was used as the negative electrode active material. Carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) were added as negative electrode binders, single-walled carbon nanotubes (SWCNT) and carbon black (SP) as negative electrode conductive agents, and water (the mass ratio of carbon-coated metal composite porous carbon material:SBR:CMC:SWCNT:SP: was 96:1.5:1.3:0.5:0.7). The mixture was homogenized using a planetary homogenizer, and the solid content was controlled at 42-45% to obtain the negative electrode slurry. The obtained negative electrode slurry was coated onto the negative electrode current collector to obtain the negative electrode sheet.
[0078] 2) Preparation of positive electrode sheet: The positive electrode is prepared by using positive electrode active material (high nickel ternary material), positive electrode conductive agent (graphene, SWCNT, SP), positive electrode binder (PVDF, polyvinylidene fluoride), and N-methylpyrrolidone NMP (the mass ratio of positive electrode active material, positive electrode conductive agent and positive electrode binder is 97:1:2) to make positive electrode slurry. The slurry is homogenized by a planetary homogenizer, and the solid content is controlled at 55-65%. The obtained positive electrode slurry is coated onto the positive electrode current collector to obtain the positive electrode sheet.
[0079] 3) Preparation of lithium-ion batteries: The process involves stacking positive and negative electrode sheets and a solid electrolyte membrane, followed by assembly, degassing, and formation. Figure 11 The square gel polymer membrane lithium battery shown.
[0080] Example 8
[0081] Example 8 uses polyacrylamide gel and a conductive agent to prepare a gel-state negative electrode. A carbon-coated metal composite porous carbon material is used as the active material. The mass ratio of conductive agent SP to polyacrylamide is 90:2:8. The mixture is dry-coated in a dry atmosphere with a dew point of -40°C. The negative electrode is then dry-coated onto copper foil to obtain the negative electrode sheet. The coating amount of the negative electrode is 21 mg / cm³. 2The positive electrode uses a porous high-nickel ternary single crystal material (LATP-coated ternary material Ni90) coated with LATP (lithium aluminum titanium phosphate), with a nickel content greater than or equal to 90%. A mesh-like positive electrode sheet is formed using PVDF as the binder and SWCNT and LITX200 as the conductive agents. The ratio of LATP-coated ternary material Ni90:PVDF:SWCNT:LITX200 is 96.8:2:0.5:0.7. Dry slurry preparation is performed under a dry atmosphere with a dew point of -40℃, followed by dry coating. Aluminum foil is used as the current collector, and the positive electrode coating amount is 50 mg / cm³. 2 The separator uses a gel electrolyte for battery assembly. 200g of liquid electrolyte is injected, filling the electrode pores of both the positive and negative electrodes. The pores are filled with non-flowing electrolyte and maintain a certain degree of elasticity, forming a semi-solid structure. Figure 11 The battery shown is fabricated as a gel-state electrode battery.
[0082] Comparative Example 1
[0083] A method for preparing porous carbon materials, wherein graphite material is prepared by etching in an alkaline solution.
[0084] Specifically, the steps are as follows: 1) First, add 2 mol of Zn(OH)2 to 1000 ml of water to prepare a 2 mol / L alkaline solution of Zn(OH)2. Then, add sample A or sample B ( Figure 1 500g of the sample (as shown in a) was added to a Zn(OH)2 solution and stirred with a mechanical stirrer for 30-60 minutes to form a mud-like solution. Then it was dried in a forced-air drying oven at 100℃ for 8 hours.
[0085] 2) The dried material obtained in step 1) was calcined at 650°C under an inert atmosphere for 2 hours;
[0086] 3) After calcination, the material was washed with 1 mol / L hydrochloric acid until neutral, and then dried to obtain the porous carbon material of Comparative Example 1.
[0087] like Figure 8 The electron micrographs show that sample A, treated only with an alkaline solution, ( Figure 8 Figure a) and sample B) Figure 8 (Figure b) The electrode has a small number of uneven pores, and the pore size is uncontrollable. The pores of sample A are 200-1000nm, and the pores of sample B are 200-1500nm, which are discretely distributed.
[0088] In summary, the porous carbon material of this invention primarily targets the modification of graphite anodes. It employs a non-metallic catalyst for directional etching of graphite, resulting in porous carbon materials with controllable pore size and uniform distribution. Furthermore, lithium metal solution is freeze-dried at low temperature using spray drying to produce nano- or micron-sized hollow spherical lithium metal particles, which are then deposited onto the surface of the porous carbon material. This results in uniform lithium metal distribution and facilitates industrialization. Building upon this, a vapor-phase carbon coating is applied to the surface of the lithium-deposited porous carbon material to enhance its electrical and safety performance, filling the technological gap in lithium metal deposition through etched pores. This material can be applied to conventional lithium-ion batteries, gel polymer membrane lithium batteries, and gel electrode lithium batteries.
[0089] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A porous carbon material, characterized in that, It contains etched holes; the etched holes are circular, with a diameter of 100 nm-4 μm and a pore volume of 1.39-1.57 cm³. 3 / g; The method for preparing the porous carbon material comprises the following steps: graphite material is prepared by etching in an alkaline solution using a catalyst; the alkaline solution is an aqueous solution of one or more of LiOH, Zn(OH)2, or Ca(OH)2; the catalyst is one or more of phosphorene, black phosphorus, lithium sulfide, boron nitride, boron phosphate, lithium phosphide, or magnesium silicate; and the mass ratio of the catalyst to the graphite material is 1%-10%.
2. The porous carbon material according to claim 1, characterized in that, The preparation method of porous carbon materials specifically includes the following steps: 1) Add the graphite material to an alkaline solution containing a catalyst, stir until homogeneous, and then dry. 2) Calcine the dried material obtained in step 1); 3) After calcination, the porous carbon material is obtained by washing and drying with an acidic solution.
3. The porous carbon material according to claim 2, characterized in that, Step 1) The graphite material is primary granular graphite and / or secondary granular graphite, with a particle size D50 ≥ 8 μm, uniform graphite particle size, and graphitization degree ≥ 95%.
4. The porous carbon material according to claim 2, characterized in that, The calcination temperature in step 2) is 350-700℃; the calcination time is 1-3h.
5. The porous carbon material according to claim 4, characterized in that, The calcination time is 2 hours.
6. A carbon-coated metal composite porous carbon material, characterized in that, The invention includes a metal composite porous carbon material and carbon coated on its surface. The metal composite porous material includes the porous carbon material according to any one of claims 1-5 and lithium metal disposed in the pores of the porous carbon material. The lithium metal accounts for 5%-50% of the volume of the pores in the metal composite porous carbon material. The amount of carbon coating in the carbon-coated metal composite porous carbon material accounts for 0.5%-3% of the mass of the metal composite porous carbon material.
7. The carbon-coated metal composite porous carbon material according to claim 6, characterized in that, In the metal composite porous carbon material, lithium metal accounts for 30% of the pore volume; the carbon coating amount in the carbon-coated metal composite porous carbon material accounts for 1.2% of the mass of the metal composite porous carbon material.
8. A method for preparing a carbon-coated metal composite porous carbon material as described in claim 6 or 7, characterized in that, Includes the following steps: 1) Lithium metal was heated to melt in an inert gas and then freeze-dried by spray to produce hollow lithium metal spheres with a diameter of 100 nm to 50 μm; 2) The porous carbon material and the lithium metal hollow spheres obtained in step 1) are mixed in an inert gas and heated to 200-450°C, held at that temperature for 4-8 hours, and then cooled to room temperature to obtain a metal composite porous carbon material; the lithium metal hollow spheres account for 7%-44% of the volume of the porous carbon material; 3) The obtained metal composite porous carbon material is subjected to carbon source gas vapor phase deposition to obtain carbon-coated metal composite porous carbon material. The temperature for carbon deposition on the surface of the metal composite porous carbon is controlled below 150℃.
9. The preparation method according to claim 8, characterized in that, Step 2) Heat to 400℃ and keep warm for 8 hours; the lithium metal hollow spheres account for 20% of the volume of the porous carbon material.
10. The preparation method according to claim 8, characterized in that, The carbon source gas mentioned in step 3) is methane or ethane.
11. A negative electrode sheet, characterized in that, It includes the porous carbon material according to any one of claims 1-5 or the carbon-coated metal composite porous carbon material according to claim 6 or 7.
12. A lithium-ion battery, characterized in that, Includes the negative electrode sheet as described in claim 11; the lithium-ion battery is a gel polymer membrane battery or a gel electrode battery.
Citation Information
Patent Citations
Silicon-carbon negative electrode material and preparation method and application thereof
CN115360331A
Electrode Forming Process for Metal-Ion Battery with Hexacyanometallate Electrode
US20130260222A1