A multi-chamber die-casting mold

By using a tapered connecting pipe and a vacuum control system in a multi-chamber die-casting mold, synchronous vacuuming of multiple chambers was achieved, solving the problems of large footprint and high maintenance difficulty of multi-chamber die-casting molds, and improving production efficiency and product quality.

CN117531974BActive Publication Date: 2026-11-24WAGON PRECISION (SUZHOU) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311570703.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-23
Publication Date
2026-11-24
Estimated Expiration
2043-11-23

AI Technical Summary

Technical Problem

Existing multi-chamber die-casting molds require the installation of multiple vacuum pumps during vacuuming, resulting in a large footprint, high maintenance difficulty, and increased costs.

Method used

Multiple molding cavities are connected by a tapered connecting pipe, and a single vacuum pump is used to simultaneously evacuate the vacuum. The vacuum level is controlled by a vacuum control system and a solenoid valve, which reduces the number of vacuum pumps, simplifies maintenance, and reduces equipment costs.

Benefits of technology

It improves the die-casting molding rate and vacuum processing efficiency, reduces equipment footprint and noise, stabilizes gas pressure, and improves the quality of molded products and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117531974B_ABST
    Figure CN117531974B_ABST
Patent Text Reader

Abstract

This invention discloses a multi-chamber die-casting mold, comprising: several upper mold groups and several lower mold groups, a driving assembly for driving the upper mold groups, and a vacuum assembly located on one side of the lower mold groups; the lower mold groups include: a first lower mold, second lower molds located on both sides of the first lower mold, and a connecting pipe connecting the first lower mold and the second lower mold; the constricted end of the connecting pipe is fixedly installed on the side of the first lower mold, and the extended end of the connecting pipe is fixedly installed on the side of the second lower mold; this invention improves the die-casting rate by setting up a die-casting mold with multiple chambers for synchronous die-casting, and uses a gradually constricting connecting pipe to connect the forming cavities of multiple die-casting molds for synchronous vacuuming, reducing the number of vacuum pumps and the number of vacuum pump maintenance required later, thereby reducing equipment costs, reducing equipment footprint, reducing noise and vibration, and simplifying the die-casting process while making efficient use of space.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to die casting molds, and more particularly to a multi-chamber die casting mold. Background Technology

[0002] A die-casting mold is a tool used to complete the die-casting process on a specialized die-casting and forging machine. The basic process of die casting is as follows: molten metal is first poured into the mold cavity at low or high speed. The mold has movable cavity surfaces, which are pressurized and forged as the molten metal cools, eliminating shrinkage cavities and porosity defects in the blank and achieving a forged, fragmented grain structure in the blank. The overall mechanical properties of the blank are significantly improved. To meet the needs of large-scale, high-volume production, multi-chamber die-casting molds are often used. Multi-chamber die-casting molds are a commonly used type of mold in the die-casting molding process. They have multiple independent forming cavities and can produce multiple die-cast parts simultaneously.

[0003] During the casting process, factors such as temperature, pressure, and flow state within the die-casting mold can affect the shape, density, and internal structure of the casting, easily leading to defects. Therefore, before the molten metal enters the forming cavity of a multi-chamber die-casting mold, the forming cavity needs to be evacuated to reduce defects such as pinholes and bubbles, improve casting quality, and reduce scrap. However, the existing method for evacuating multiple cavities in a multi-chamber die-casting mold involves installing a vacuum pump in each cavity to achieve rapid vacuuming. However, installing multiple vacuum pumps increases the footprint of the entire device and the difficulty of maintenance, thus increasing maintenance costs.

[0004] Therefore, it is necessary to design a multi-chamber die-casting mold to address the shortcomings of the above-mentioned problems. Summary of the Invention

[0005] This invention overcomes the shortcomings of the prior art and provides a multi-chamber die-casting mold.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: a multi-chamber die-casting mold, comprising: a plurality of upper mold groups and a plurality of lower mold groups, a driving assembly for driving the plurality of upper mold groups, and a vacuum assembly located on one side of the plurality of lower mold groups, wherein the driving assembly drives the plurality of upper mold groups and the plurality of lower mold groups to fit together and seal to form a cavity;

[0007] The lower module includes: a first lower mold, a second lower mold located on both sides of the first lower mold, and a connecting pipe connecting the first lower mold and the second lower mold; the connecting pipe is a tapered pipe, with the constricted end of the connecting pipe fixedly installed on the side of the first lower mold and the extended end of the connecting pipe fixedly installed on the side of the second lower mold;

[0008] The upper module includes: a plurality of upper molds, and a fixing frame located on one side of the plurality of upper molds; the plurality of upper molds correspond one-to-one with the first lower mold and the second lower mold, and the plurality of upper molds are fixedly installed on the fixing frame.

[0009] In a preferred embodiment of the present invention, both the first lower mold and the second lower mold are provided with mold grooves, the first lower mold and the upper mold are sealed together to form a first molding cavity, and the second lower mold and the upper mold are sealed together to form a second molding cavity.

[0010] In a preferred embodiment of the present invention, the angle between the contracting wall of the tapered connecting pipe and its central axis is 0 to 70°.

[0011] In a preferred embodiment of the present invention, the vacuum component is a vacuum pump, and its suction end is connected to the mold groove of the first lower mold.

[0012] In a preferred embodiment of the present invention, the driving component is a hydraulic cylinder, the output end of which is fixed to the middle position of the fixed frame, thereby driving the fixed frame to move up and down.

[0013] In a preferred embodiment of the present invention, a base is installed below the plurality of lower modules, and the plurality of lower modules are embedded in the base.

[0014] In a preferred embodiment of the present invention, the bottom of a plurality of first lower molds and a plurality of second lower molds are provided with inlets for molten metal to enter.

[0015] In a preferred embodiment of the present invention, solenoid valves are installed at both ends of the connecting pipe.

[0016] In a preferred embodiment of the present invention, the vacuum assembly is equipped with a vacuum control system, and the vacuum control system controls the opening or closing of the solenoid valve to control the vacuum level of the die-casting mold.

[0017] In a preferred embodiment of the present invention, the vacuum control system includes: a first pressure sensor, a second pressure sensor, a first humidity sensor, a second humidity sensor, a controller, a data collection module, and a signal transmission module;

[0018] Both the first pressure sensor and the first humidity sensor are installed on the first lower mold to detect the pressure and humidity inside the first molding cavity;

[0019] Both the second pressure sensor and the second humidity sensor are installed on the second lower mold to detect the pressure and humidity inside the second molding cavity;

[0020] The signal transmission module is used to transmit signals between the first pressure sensor, the second pressure sensor, the first humidity sensor, the second humidity sensor, the controller, and the data collection module;

[0021] The data collection module collects the pressure and humidity detected by the first pressure sensor, the second pressure sensor, the first humidity sensor, and the second humidity sensor, and transmits them to the controller for processing;

[0022] The controller is equipped with a data processing module, which is used to process the data collected by the data collection module and control the opening or closing of the solenoid valve.

[0023] This invention addresses the shortcomings of the prior art and has the following beneficial effects:

[0024] (1) This invention provides a multi-chamber die casting mold. By setting multiple chambers in the die casting mold for synchronous die casting, the die casting rate is improved. The forming cavities of multiple die casting molds are connected by a gradually narrowing connecting pipe, and the vacuum process is carried out synchronously, reducing the number of vacuum pumps and the difficulty of vacuum pump maintenance in the later stage. This reduces equipment costs, reduces the equipment footprint, reduces noise and vibration, and simplifies the die casting process while making efficient use of space.

[0025] (2) By setting up a gradually narrowing connecting pipe, the present invention creates a pressure difference between adjacent molding cavities. In conjunction with the vacuuming process, the airflow speed is further increased. During the flow, the gas will carry away more residual gas, thereby reducing the amount of residual gas in the cavity, which helps to improve the efficiency of vacuuming and thus increase the die casting rate.

[0026] (3) By setting up a gradually narrowing connecting pipe, the present invention utilizes the fact that the gas flow rate of the gradually narrowing connecting pipe is inversely proportional to the pipe diameter. When the gas flow rate increases, the kinetic energy of the gas increases. The increase in kinetic energy will offset part of the pressure difference generated when the gas flows from the second forming cavity to the first forming cavity, thereby stabilizing the gas pressure, avoiding large gas pressure fluctuations, reducing gas residue, ensuring the stability of the vacuum degree, and thus ensuring the quality of the molded product. Attached Figure Description

[0027] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0028] Figure 1 This is a perspective structural diagram of a preferred embodiment of the present invention;

[0029] Figure 2 This is a rear view schematic diagram of the overall structure of a preferred embodiment of the present invention;

[0030] Figure 3 This is a schematic diagram of the lower module structure according to a preferred embodiment of the present invention;

[0031] Figure 4 This is a schematic diagram of the structure of the first molding cavity and the second molding cavity according to a preferred embodiment of the present invention;

[0032] Figure 5 This is a schematic diagram of the connecting pipe according to a preferred embodiment of the present invention;

[0033] Figure 6 These are schematic diagrams illustrating the pressure changes in the cavity of the preferred embodiments of the present invention, namely Embodiments 1 to 8.

[0034] In the diagram: 1. Upper module; 2. Lower module; 3. First lower mold; 4. Second lower mold; 5. Connecting pipe; 6. Upper mold; 7. Fixing frame; 8. First molding cavity; 9. Second molding cavity; 10. Vacuum pump; 11. Hydraulic cylinder. Detailed Implementation

[0035] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0036] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein. Therefore, the scope of protection of the invention is not limited to the specific embodiments disclosed below.

[0037] In the description of this application, it should be understood that the terms "center," "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicating orientation or positional relationships based on the orientation or positional relationships shown in the accompanying drawings, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as limiting the scope of protection of this application. Furthermore, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, features defined with "first," "second," etc., may explicitly or implicitly include one or more of that feature. In the description of this invention, unless otherwise stated, "a plurality of" means two or more.

[0038] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to fixed connections, detachable connections, or integral connections; they can refer to mechanical connections or electrical connections; they can refer to direct connections or indirect connections through an intermediate medium; and they can refer to the internal communication between two components. Those skilled in the art will understand the specific meaning of the above terms in this application based on the specific circumstances.

[0039] like Figure 1 , Figure 2 and Figure 3 As shown, a multi-chamber die-casting mold includes: a plurality of upper mold groups 1 and a plurality of lower mold groups 2, a drive assembly for driving the plurality of upper mold groups 1, and a vacuum assembly located on one side of the plurality of lower mold groups 2. The drive assembly drives the plurality of upper mold groups 1 and the plurality of lower mold groups 2 to fit together and seal to form a cavity.

[0040] The lower module 2 includes: a first lower mold 3, a second lower mold 4 located on both sides of the first lower mold 3, and a connecting pipe 5 connecting the first lower mold 3 and the second lower mold 4; the connecting pipe 5 is a tapered pipe, with the constricted end of the connecting pipe 5 fixedly installed on the side of the first lower mold 3 and the extended end of the pipe fixedly installed on the side of the second lower mold 4.

[0041] It is worth mentioning that the connecting pipe 5 is used to connect the first lower mold 3 and the second lower mold 4 located on both sides of the first lower mold 3, so as to ensure the vacuum treatment of the die-casting mold by the subsequent vacuum assembly;

[0042] The upper module 1 includes: a plurality of upper molds 6, and a fixing frame 7 located on one side of the plurality of upper molds 6; the plurality of upper molds 6 correspond one-to-one with the first lower mold 3 and the second lower mold 4, and the plurality of upper molds 6 are fixedly installed on the fixing frame 7;

[0043] like Figure 4 As shown, mold grooves are provided in both the first lower mold 3 and the second lower mold 4. The first lower mold 3 and the upper mold 6 are sealed together to form the first forming cavity 8, and the second lower mold 4 and the upper mold 6 are sealed together to form the second forming cavity 9, so as to facilitate the subsequent injection of molten metal to form a die casting.

[0044] The first molding cavity 8 formed by the first lower mold 3 and the upper mold 6 will create a pressure difference with the second molding cavity 9 formed by the second lower mold 4 and the upper mold 6. The gas in the second molding cavity 9 formed by the second lower mold 4 will enter the first molding cavity 8 formed by the first lower mold 3 through the connecting pipe 5 and be jointly extracted by the vacuum pump 10, so as to achieve the purpose of vacuum treatment of the three molding cavities at the same time, reduce the number of vacuum pumps 10, reduce the number of maintenance of vacuum pumps 10 in the later stage, thereby reducing equipment costs, reducing equipment footprint, reducing noise and vibration, and simplifying the die casting process while making efficient use of space.

[0045] The bottom of several first lower molds 3 and several second lower molds 4 are provided with inlets for molten metal to enter;

[0046] Considering that if there is gas in the molding cavity during the process of injecting molten metal into the molding cavity, it may cause the generation of bubbles or pores, the suction end of the vacuum pump 10 is connected to the mold groove of the first lower mold 3 to perform vacuum treatment on the formed molding cavity, the gas in the molding cavity is discharged, the generation of bubbles and pores is reduced, and the density and surface quality of the molded product are improved.

[0047] A base is installed at the lower position of several lower modules 2, and several lower modules 2 are embedded in the base.

[0048] It should be noted that when die casting is required, the drive assembly drives the fixed frame 7 to move towards the lower mold group 2 until the upper mold 6 is located in the first lower mold 3 and the second lower mold 4 in the lower mold group 2 and is sealed and fitted. Since the first lower mold 3, the second lower mold 4 and the upper mold 6 all have mold grooves, a forming cavity is formed. The vacuum pump 10 is controlled to perform vacuum treatment on the forming cavity formed by the first lower mold 3 and the upper mold group 1. The two second lower molds 4 are connected to the first lower mold 3 through the connecting pipe 5. One vacuum pump 10 can perform simultaneous vacuum treatment on the three forming cavities, reducing the number of vacuum pumps 10 and the number of vacuum pumps 10 to be maintained later, thereby reducing equipment costs. The molten metal enters the forming cavity through the bottom feed port of the first lower mold 3 and the second lower mold 4, and then is die-cast to obtain the required die-cast part.

[0049] The driving component is a hydraulic cylinder 11. The output end of the hydraulic cylinder 11 is fixed to the middle position of the fixed frame 7, driving the fixed frame 7 to move up and down.

[0050] Solenoid valves are installed at both ends of the connecting pipe 5.

[0051] Because vacuum treatment of the molding cavity can improve the density and surface quality of the molded product, it is necessary to ensure the vacuum level in the molding cavity. This can reduce the obstruction of gas to metal filling, facilitate the filling of molten metal, and improve the dimensional and shape accuracy of the molded product. Since the molding cavity of die casting is a series of interconnected molding cavities, and a single vacuum pump 10 is used for synchronous vacuum treatment, it is necessary to set up a connecting pipe 5.

[0052] like Figure 5 As shown, in this invention, the angle between the contraction wall of the tapered connecting pipe 5 and its central axis is 0 to 70°, thereby controlling the air pressure in the first forming cavity 8 to be stable.

[0053] By changing the connecting pipe 5 with the shrinkage wall surface at different angles to its central axis, the vacuuming rate between the first forming cavity 8 and the second forming cavity 9 will be different.

[0054] Example 1:

[0055] Prepare two identical first and second chambers, with the initial atmospheric pressure inside. Select a connecting pipe 5 with the angle between the contraction wall and its central axis being 0°, i.e., a straight pipe. The length of the connecting pipe 5 is 15cm and the maximum inner diameter is 5cm. 2XZ type direct-drive vacuum pump 10, data logger, power supply, pressure sensor and gas flow rate sensor.

[0056] The constricted end of the connecting pipe 5 is fixed to the first cavity and connected to it. The other end of the connecting pipe 5 is fixed to the second cavity and connected to it. Pressure sensors are installed in the first cavity and the second cavity respectively. Gas flow rate sensors are installed in the connecting pipe 5. The pumping end of the 2XZ type direct-drive vacuum pump 10 is connected to the first cavity. The power is turned on, and the 2XZ type direct-drive vacuum pump 10 is controlled to evacuate the first cavity for 0.5 minutes. The data logger records the pressure values ​​in the first cavity and the second cavity, determines whether 50 kPa (absolute pressure) has been reached, the magnitude of the gas flow rate in the connecting pipe 5, and analyzes the pressure fluctuation and stability in the first cavity and the second cavity within 0.5 minutes.

[0057] Example 2: Prepare two identical first and second cavities, with the initial atmospheric pressure inside. Select a connecting pipe 5 with an angle of 10° between the contraction wall surface and its central axis, i.e., a gradually narrowing connecting pipe 5. The length of the connecting pipe 5 is 15cm, the maximum inner diameter is 5cm, and the length of the contraction end of the connecting pipe 5 is 5cm. 2XZ type direct-drive vacuum pump 10, data logger, power supply, pressure sensor and gas flow rate sensor are also included.

[0058] The constricted end of the connecting pipe 5 is fixed to the first cavity and connected to it. The other end of the connecting pipe 5 is fixed to the second cavity and connected to it. Pressure sensors are installed in the first cavity and the second cavity respectively. Gas flow rate sensors are installed in the connecting pipe 5. The pumping end of the 2XZ type direct-drive vacuum pump 10 is connected to the first cavity. The power is turned on, and the 2XZ type direct-drive vacuum pump 10 is controlled to evacuate the first cavity for 0.5 minutes. The data logger records the pressure values ​​in the first cavity and the second cavity, determines whether 50 kPa (absolute pressure) has been reached, the magnitude of the gas flow rate in the connecting pipe 5, and analyzes the pressure fluctuation and stability in the first cavity and the second cavity within 0.5 minutes.

[0059] Example 3 is basically the same as Example 2, except that a connecting pipe 5 with a 20° angle between the contraction wall and its central axis is selected. During the vacuuming process, the pressure values ​​in the first and second cavities after 0.5 minutes, the gas flow velocity in the connecting pipe 5, and the pressure fluctuations and stability in the first and second cavities within 0.5 minutes are recorded.

[0060] Example 4 is basically the same as Example 2, except that a connecting pipe 5 with a 30° angle between the contraction wall and its central axis is selected. During the vacuuming process, the pressure values ​​in the first and second cavities after 0.5 minutes are recorded, as well as the gas flow rate in the connecting pipe 5. The fluctuations and stability of the pressure in the first and second cavities within 0.5 minutes are analyzed.

[0061] Example 5 is basically the same as Example 2, except that a connecting pipe 5 with a 40° angle between the contraction wall and its central axis is selected. During the vacuuming process, the pressure values ​​in the first and second cavities after 0.5 minutes are recorded, as well as the gas flow rate in the connecting pipe 5. The fluctuations and stability of the pressure in the first and second cavities within 0.5 minutes are analyzed.

[0062] Example 6 is basically the same as Example 2, except that a connecting pipe 5 with a 50° angle between the contraction wall and its central axis is selected. During the vacuuming process, the pressure values ​​in the first and second cavities after 0.5 minutes are recorded, as well as the gas flow rate in the connecting pipe 5. The fluctuations and stability of the pressure in the first and second cavities within 0.5 minutes are analyzed.

[0063] Example 7 is basically the same as Example 2, except that a connecting pipe 5 with a 60° angle between the contraction wall and its central axis is selected. During the vacuuming process, the pressure values ​​in the first and second cavities after 0.5 minutes are recorded, as well as the gas flow rate in the connecting pipe 5. The fluctuations and stability of the pressure in the first and second cavities within 0.5 minutes are analyzed.

[0064] Example 8 is basically the same as Example 2 in operation, except that a connecting pipe 5 with a 70° angle between the contraction wall and its central axis is selected. During the vacuuming process, the pressure values ​​in the first and second cavities after 0.5 minutes are recorded, as well as the gas flow rate in the connecting pipe 5. The fluctuations and stability of the pressure in the first and second cavities within 0.5 minutes are analyzed.

[0065] Comparative Example 1:

[0066] Prepare two identical first and second chambers, with the initial atmospheric pressure inside. Include a 2XZ type direct-drive vacuum pump 10, a data logger, a power supply, a pressure sensor, and a gas flow rate sensor. Also include a connecting pipe 5 with a constricted wall surface at a 30° angle to its central axis (i.e., a gradually constricting connecting pipe 5). Select a connecting pipe 5 with a length of 15cm, a maximum inner diameter of 5cm, and a constricted end length of 7.5cm. The minimum inner diameter will be smaller than the minimum inner diameter of the connecting pipe 5 in Example 4.

[0067] The constricted end of the connecting pipe 5 is fixed to the first cavity and connected to it. The other end of the connecting pipe 5 is fixed to the second cavity and connected to it. Pressure sensors are installed in the first cavity and the second cavity respectively. Gas flow rate sensors are installed in the connecting pipe 5. The pumping end of the 2XZ type direct-drive vacuum pump 10 is connected to the first cavity. The power is turned on, and the 2XZ type direct-drive vacuum pump 10 is controlled to evacuate the first cavity for 0.5 minutes. The data logger records the pressure values ​​in the first cavity and the second cavity, determines whether 50 kPa (absolute pressure) has been reached, the magnitude of the gas flow rate in the connecting pipe 5, and analyzes the pressure fluctuation and stability in the first cavity and the second cavity within 0.5 minutes.

[0068] Comparative Example 2 is basically the same as Comparative Example 1, except that the length of the connecting pipe 5 is 15cm, the maximum inner diameter is 5cm, the length of the contracted end of the connecting pipe 5 is 2.5cm, and the minimum inner diameter is larger than the minimum inner diameter of the connecting pipe 5 in Example 4. During the vacuuming process, the pressure values ​​in the first and second cavities after 0.5min, the gas flow velocity in the connecting pipe 5, and the fluctuation and stability of the pressure in the first and second cavities within 0.5min are recorded.

[0069] Table 1 shows the pressure values ​​and stability changes in the first and second chambers after 0.5 minutes.

[0070]

[0071]

[0072] In summary, as Figure 6 As shown, the pressure values ​​of the first and second cavities change with the increase of the angle between the constricted wall of the connecting pipe 5 and its central axis. That is, when the angle between the constricted wall of the connecting pipe 5 and its central axis is 0° to 30°, the pressure values ​​of the first and second cavities gradually decrease within a specified time. When the angle between the constricted wall of the connecting pipe 5 and its central axis is 30° to 70°, the pressure values ​​of the first and second cavities gradually increase within a specified time. This indicates that the vacuuming rate is fastest when the angle between the constricted wall of the connecting pipe 5 and its central axis is 30°.

[0073] Although the gas velocity through the constricted end of the connecting pipe 5 gradually increases as the angle between the constricted wall and its central axis changes from 0 to 70°, the smaller diameter of the constricted end of the connecting pipe 5 prevents the gas in the second cavity from passing through quickly, thus slowing down the gas flow efficiency in the second cavity. Therefore, when the angle between the constricted wall and its central axis of the connecting pipe 5 is between 30 and 70°, the pressure values ​​in the first and second cavities will gradually increase within a specified time.

[0074] The reason why the air pressure in the second cavity remains stable during the process of the angle between the constricted wall of the connecting pipe 5 and its central axis changing from 0 to 70° is because the end of the connecting pipe 5 with the maximum diameter is connected to the second cavity. The maximum diameter of the connecting pipe 5 serves as the gas output end, and since the diameter remains constant, its impact on the air pressure in the second cavity is relatively small. The reason why the air pressure stability in the first cavity shows a peak change is because the diameter of the constricted end of the connecting pipe 5 gradually decreases, which increases the gas velocity. Although the increase in gas velocity increases the kinetic energy of the gas, and the increase in kinetic energy will offset part of the pressure difference generated when the gas flows into the first cavity, thus achieving the effect of stabilizing the air pressure in the first cavity, if the gas velocity is too high, the airflow flowing into the first cavity will impact in the first cavity, which will be unstable or eddy currents will appear, leading to unstable air pressure. This may result in gas residue in the cavity, affecting the purification effect of the process.

[0075] A stable gas pressure in the cavity can help improve the pumping efficiency of the vacuum pump 10 and enhance the purification effect of the process. At the same time, a stable gas pressure can reduce the workload of the vacuum pump 10 and extend its service life. Therefore, in the above embodiments, Embodiment 4 has the best overall comparative effect. That is, when the angle between the contracted wall of the connecting pipe 5 and its central axis is 30°, the pressure values ​​of the first cavity and the second cavity are at their lowest values ​​and are below 50 kPa (absolute pressure). Therefore, the vacuuming rate is the highest at this time, and the gas pressure stability in the first cavity is relatively high, which can better reduce the residual gas in the cavity.

[0076] Comparing Comparative Example 1 and Example 4, it can be concluded that when the angle between the constricted wall surface of the tapered connecting pipe 5 and its central axis is 30°, increasing the length of the constricted wall surface of the tapered connecting pipe 5 will result in the minimum inner diameter of the tapered connecting pipe 5 being smaller than the minimum inner diameter of the connecting pipe 5 in Example 4. Therefore, during the experiment, the gas passes through the connecting pipe 5 in Comparative Example 1 at a faster speed, and the airflow flowing towards the first cavity will impact in the first cavity, causing instability or eddies in the first cavity, resulting in unstable air pressure in the first cavity.

[0077] Comparing Comparative Example 2 and Example 4, it can be concluded that when the angle between the contraction wall of the tapered connecting pipe 5 and its central axis is 30°, reducing the length of the contraction wall of the tapered connecting pipe 5 will result in the minimum inner diameter of the tapered connecting pipe 5 being greater than the minimum inner diameter of the connecting pipe 5 in Example 4. Therefore, during the experiment, the gas passes through the connecting pipe 5 in Comparative Example 1 at a slower speed, which ensures that the kinetic energy of the airflow will offset part of the pressure difference generated when the gas flows from the second cavity to the first cavity, making the gas pressure in the first cavity more stable. However, compared with Example 4, the gas pressure stability of its first cavity is slightly lower.

[0078] In this invention, the vacuum assembly is equipped with a vacuum control system, and the vacuum control system controls the opening or closing of the solenoid valve to control the vacuum level of the die-casting mold.

[0079] In this invention, the vacuum control system includes: a first pressure sensor, a second pressure sensor, a first humidity sensor, a second humidity sensor, a controller, a data collection module, and a signal transmission module;

[0080] Both the first pressure sensor and the first humidity sensor are installed on the first lower mold 3 to detect the pressure and humidity inside the first molding cavity 8.

[0081] The second pressure sensor and the second humidity sensor are both installed on the second lower mold 4 to detect the pressure and humidity inside the second molding cavity 9.

[0082] The signal transmission module is used to transmit signals between the first pressure sensor, the second pressure sensor, the first humidity sensor, the second humidity sensor, the controller, and the data collection module;

[0083] The data collection module collects the pressure and humidity detected by the first pressure sensor, the second pressure sensor, the first humidity sensor, and the second humidity sensor, and transmits them to the controller for processing;

[0084] The controller is equipped with a data processing module, which is used to process the data collected by the data collection module and control the opening or closing of the solenoid valve.

[0085] In use, the hydraulic cylinder 11 drives the upper mold 1 to move towards the lower mold 2 and seals with it. That is, the first lower mold 3 and the upper mold 6 are sealed together to form the first molding cavity 8, and the second lower mold 4 and the upper mold 6 are sealed together to form the second molding cavity 9. The vacuum control system controls the solenoid valve to open and controls the vacuum pump 10 to evacuate the first molding cavity 8. The gas pressure in the first molding cavity 8 decreases, and the gas in the second molding cavity 9, which is connected to the first molding cavity 8, flows towards the first molding cavity 8 through the connecting pipe 5. Thus, both the first molding cavity 8 and the second molding cavity 9 are evacuated. The vacuum control system controls the solenoid valve to close. Then, molten metal is injected into the first molding cavity 8 and the second molding cavity 9 through the feed port for die casting.

[0086] Based on the preferred embodiments of the present invention described above, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.

Claims

1. A multi-chamber die-casting mold, comprising: A plurality of upper modules and a plurality of lower modules, a drive assembly for driving the plurality of upper modules, and a vacuum assembly located on one side of the plurality of lower modules, characterized in that the drive assembly drives the plurality of upper modules and the plurality of lower modules to fit together and seal to form a cavity; The lower module includes: a first lower mold, a second lower mold located on both sides of the first lower mold, and a connecting pipe connecting the first lower mold and the second lower mold; the connecting pipe is a tapered pipe, with the constricted end of the connecting pipe fixedly installed on the side of the first lower mold and the extended end of the pipe fixedly installed on the side of the second lower mold; The upper module includes: a plurality of upper molds, and a fixing frame located on one side of the plurality of upper molds; the plurality of upper molds correspond one-to-one with the first lower mold and the second lower mold, and the plurality of upper molds are fixedly installed on the fixing frame; Both the first lower mold and the second lower mold have mold grooves. The first lower mold and the corresponding upper mold are sealed together to form a first molding cavity, and the second lower mold and the corresponding upper mold are sealed together to form a second molding cavity. The vacuum component is a vacuum pump, and the pumping end of the vacuum pump is connected to the mold groove of the first lower mold, so that the gas in the second molding cavity enters the first molding cavity through the tapered connecting pipe and is jointly extracted by the vacuum pump. Wherein, the first molding cavity serves as a gas confluence cavity when multiple molding cavities are evacuated together, and the second lower mold is connected to the first lower mold through corresponding tapered connecting pipes; The angle between the contracting wall of the tapering connecting pipe and its central axis is 30°.

2. The multi-chamber die-casting mold according to claim 1, characterized in that: The drive component is a hydraulic cylinder, and the output end of the hydraulic cylinder is fixed to the middle position of the fixed frame, driving the fixed frame to move up and down.

3. The multi-chamber die-casting mold according to claim 1, characterized in that: A base is installed below several lower modules, and several lower modules are embedded in the base.

4. A multi-chamber die-casting mold according to claim 1, characterized in that: The bottom of several first lower dies and several second lower dies are provided with inlets for molten metal to enter.

5. A multi-chamber die-casting mold according to claim 1, characterized in that: Solenoid valves are installed at both ends of the connecting pipe.

6. A multi-chamber die-casting mold according to claim 5, characterized in that: The vacuum assembly is equipped with a vacuum control system, which controls the opening and closing of the solenoid valve to control the vacuum level of the die-casting mold.

7. A multi-chamber die-casting mold according to claim 6, characterized in that: The vacuum control system includes: a first pressure sensor, a second pressure sensor, a first humidity sensor, a second humidity sensor, a controller, a data acquisition module, and a signal transmission module; Both the first pressure sensor and the first humidity sensor are installed on the first lower mold to detect the pressure and humidity inside the first molding cavity; The second pressure sensor and the second humidity sensor are both installed on the second lower mold to detect the pressure and humidity inside the second molding cavity; The signal transmission module is used to transmit signals between the first pressure sensor, the second pressure sensor, the first humidity sensor, the second humidity sensor, the controller, and the data collection module; The data collection module collects the pressure and humidity detected by the first pressure sensor, the second pressure sensor, the first humidity sensor, and the second humidity sensor, and transmits them to the controller for processing; The controller is equipped with a data processing module, which is used to process the data collected by the data collection module and control the opening or closing of the solenoid valve.

Citation Information

Patent Citations

  • Vacuum pumping system for die cavities of die-casting dies

    CN104209492A

  • Sucker device self-adaptive to multi-size substrates

    CN116489889A

  • Vacuum communication assembly and PVD (Physical Vapor Deposition) system

    CN215209612U

  • Die casting structure for spectacle frame

    CN219766741U