A smelting method for improving production efficiency and yield of titanium alloy ingot

By adjusting the smelting parameters of the VAR method and the electrode inverted charging technology, the problem of excessively thick flash at the head of titanium alloy ingots was solved, improving production efficiency and yield, and achieving a safe and stable smelting process.

CN117535539BActive Publication Date: 2026-11-24XIAN SUPERCRYSYAL SCI TECH DEV CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311336157.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-16
Publication Date
2026-11-24
Estimated Expiration
2043-10-16

AI Technical Summary

Technical Problem

When using the existing VAR method to prepare industrially common large-sized titanium alloy ingots, the excessively thick flash at the head leads to problems such as large processing volume, low production efficiency, and low yield.

Method used

By adjusting the melting current, voltage, and arc stabilization current during the vacuum self-consuming electric arc furnace melting process, especially by reducing them four times at the end of the melting process and switching to AC stirring when the arc is extinguished, combined with the inverted electrode loading during the second or third melting process, the phenomenon of the molten pool not reaching the edge is reduced, and the thickness of the flash is controlled to be within 20mm.

Benefits of technology

It significantly reduces the amount of processing required for titanium alloy ingots, increases production efficiency by more than 50%, and improves the yield, while ensuring the safety and uniformity of the composition during smelting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117535539B_ABST
    Figure CN117535539B_ABST
Patent Text Reader

Abstract

This invention discloses a smelting method to improve the production efficiency and yield of titanium alloy ingots, comprising the following steps: 1) electrode preparation; 2) primary smelting; 3) primary ingot processing; 4) secondary or tertiary smelting; 5) processing, sampling, and analysis. Each step involves strict control of relevant parameters, especially the primary smelting, which is achieved by adjusting the parameters at the end of the arc termination process. Specifically, the smelting current is reduced by 1 kA per minute, the voltage by 1 V, and the arc-stabilizing current by 1 A, for a total of four reductions until the smelting is complete. During arc termination, AC stirring is used for arc stabilization, with a stirring cycle of 15-30 seconds. When preparing industrially common large-sized primary ingots (Φ500mm-Φ640mm), this invention significantly reduces the thickness of the flash at the head compared to existing technologies. Therefore, it requires less processing and significantly improves the production efficiency and yield of titanium alloy ingots. Furthermore, the final titanium alloy ingot composition meets the requirements of GB / T3620.1 standard and is uniformly homogeneous.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of titanium alloy preparation technology, specifically relating to a smelting method for improving the production efficiency and yield of titanium alloy ingots. Background Technology

[0002] Titanium alloys are widely used in aerospace, petroleum, and chemical industries due to their excellent properties such as high specific strength, corrosion resistance, shape memory, and biocompatibility. Currently, the main methods for melting titanium alloys include vacuum arc remelting (VAR), non-consumable vacuum arc remelting (NC), cold hearth melting (CHM), cold crucible melting (CCM), and electroslag remelting (ESR). Because of its low power consumption, fast melting speed, and good quality reproducibility, the VAR method produces ingots with good crystalline structure and uniform chemical composition, making it the mainstream technology for titanium alloy ingot preparation. It typically involves two or three melting cycles.

[0003] In the first melting process, the consumable electrode is composed of electrode blocks pressed from a mixture of sponge titanium and intermediate alloy, forming a physically bonded block. Therefore, during this process, impurities in the electrode blocks continuously volatilize upon heating. Under the influence of the arc-stabilizing stirring magnetic field, floating matter and impurities in the molten pool diffuse outwards from the center of the water-cooled copper crystallizer. Upon encountering the inner wall of the crystallizer, they cool, solidify, and adhere to the ingot surface. As melting progresses, the outer shell formed by impurities and volatilized substances rises, eventually resulting in a high and thick flash at the end of the melting process. To address this, at the end of the melting process, the melting current, voltage, and arc-stabilizing current are typically reduced to shallow the molten pool and weaken the stirring, preventing safety accidents caused by severe arc creep and spatter. While this method can reduce the height of the flash to some extent, the reduced melting current and the reduced arc stabilization current exacerbate the problem of the molten pool not reaching the edge, resulting in excessive flash thickness. This problem becomes particularly severe as the ingot size increases, leading to a large flash thickness at the head of the primary ingot (the ingot produced by a single melting process). This is especially true when preparing industrially common larger-sized primary ingots (Φ500mm~Φ640mm), where the flash thickness can reach over 40mm. In subsequent primary ingot processing, this flash must be completely removed, resulting in a large machining workload, low production efficiency, and a significant impact on material utilization.

[0004] In view of this, this invention is hereby proposed. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide a smelting method to improve the production efficiency and yield of titanium alloy ingots. It mainly solves the problem that the flash at the head of the commonly used industrial large-size (Φ500mm~Φ640mm) primary ingot prepared by the existing VAR method is too thick, resulting in large processing volume, low production efficiency and low yield.

[0006] The objective of this invention is achieved through the following technical solution:

[0007] This invention provides a smelting method for improving the production efficiency and yield of titanium alloy ingots, comprising the following steps:

[0008] Step 1: Electrode Preparation

[0009] The constituent raw materials are determined according to the chemical composition of the target titanium alloy ingot. Then, each constituent raw material is weighed according to the mass percentage and mixed evenly before being pressed into electrode blocks. Then, several electrode blocks are welded together to form an electrode.

[0010] Step 2: First Melting

[0011] The electrode obtained in step one is used as a consumable electrode. Under set parameters, the consumable electrode is smelted once in a vacuum consumable arc furnace to finally obtain a primary ingot.

[0012] Step 3: Primary Ingot Processing

[0013] The flash at the head of the primary ingot prepared in step two is removed by machine.

[0014] Step 4: Secondary or tertiary smelting

[0015] The primary ingot obtained after step three is used as a consumable electrode and then remelted in a vacuum consumable arc furnace to obtain a secondary ingot. When loading the furnace, the primary ingot must be inverted, i.e., head down. If a third remelting is to be performed, the secondary ingot is loaded into the furnace with its head upside down.

[0016] Step 5: Processing, Sampling and Analysis

[0017] The titanium alloy ingot obtained from the final melting in step four is processed to the target size, and samples are taken for analysis. If the analysis results meet the requirements of GB / T3620.1 standard and the composition is uniform, the finished titanium alloy ingot is qualified; otherwise, it is unqualified.

[0018] Furthermore, the parameters set during the first melting in step two are as follows: melting current is 16.0KA~22.0KA, melting voltage is 33.0V~36.0V, arc stabilization current is DC 18.0A~20.0A, and 50kg~100kg of electrode is reserved at the end of melting for arc termination.

[0019] Furthermore, during the arc termination of the first melting process in step two, the melting current is required to decrease by 1 kA, the voltage by 1 V, and the arc stabilization current by 1 A per minute, for a total of four reductions, until the melting process is completed.

[0020] Furthermore, in step two, during the arc-extinguishing process of a single melting operation, the entire arc-extinguishing process takes 4 to 6 minutes.

[0021] Furthermore, during the arc extinguishing process in step two, the arc stabilizing current is changed from DC to AC, and the stirring cycle is 15s to 30s.

[0022] Furthermore, the thickness of the flash of the ingot obtained after one melting in step two is within 20mm.

[0023] Furthermore, the parameters set during the secondary melting in step four are as follows: melting current of 18.0KA~28.0KA, melting voltage of 29.0V~40.0V, arc stabilization current of AC 10.0A~25.0A, and stirring cycle of 15s~60s.

[0024] Furthermore, the parameters set for the three melting processes in step four are as follows: melting current of 20.0KA to 28.0KA, melting voltage of 30.0V to 40.0V, arc stabilization current of AC 15.0A to 25.0A, and stirring cycle of 15s to 60s.

[0025] Furthermore, the smelting method is used to prepare titanium alloy primary ingots with dimensions of Φ500mm to Φ640mm.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The VAR melting method provided by this invention reduces the molten pool depth, weakens stirring, and reduces flash height by adjusting the melting current, voltage, and arc-stabilizing current at the end of the arc termination during the first melting stage. Simultaneously, the reduced voltage shortens the arc and weakens arc climbing, ensuring safe and stable melting. Furthermore, the use of AC arc stabilization during arc termination ensures thorough stirring of the molten pool, improving the situation where the molten pool doesn't reach the edge, and avoids the arc deviation problem caused by DC stirring. This significantly reduces the problem of excessively thick flash at the head of commonly used industrial ingots with dimensions of Φ500mm to Φ640mm. Compared to existing melting methods, the flash thickness of the first ingot obtained by this invention can be controlled to within 20mm, reducing the processing weight of a single ingot from approximately 10kg to below 4kg. Therefore, the processing efficiency of the first ingot is increased by more than 50%, thus shortening the cycle required for preparing titanium alloy ingots and improving the yield of titanium alloy ingots. Attached Figure Description

[0028] The accompanying drawings are incorporated in and form part of this specification, and together with the description serve to explain the principles of the invention.

[0029] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0030] Figure 1 This is a flowchart of the smelting method of the present invention;

[0031] Figure 2 This is a photograph of the flash on the head of the ingot obtained after one melting in Embodiment 1 of the present invention;

[0032] Figure 3 This is a comparative example of Embodiment 1 of the present invention, showing the flash on the head of an ingot obtained after a single melting process using the conventional VAR method. Detailed Implementation

[0033] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numbers in different drawings denote the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Rather, they are merely examples of apparatuses consistent with some aspects of the invention as detailed in the appended claims.

[0034] To enable those skilled in the art to better understand the technical solutions of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments.

[0035] Please see Figure 1 This invention provides a smelting method for improving the production efficiency and yield of titanium alloy ingots, specifically including the following steps:

[0036] Step 1: Electrode Preparation

[0037] The raw materials are determined based on the chemical composition of the target titanium alloy ingot. Each raw material is weighed according to its mass percentage, mixed evenly, and then pressed into an electrode block. Several electrode blocks are then welded together to form an electrode.

[0038] Step 2: First Melting

[0039] The electrode obtained in step one is used as a consumable electrode. Under set parameters, the consumable electrode is smelted once in a vacuum consumable arc furnace to finally obtain a primary ingot.

[0040] Specifically, the parameters set for a single melting process are as follows: melting current is 16.0KA~22.0KA, melting voltage is 33.0V~36.0V, and arc stabilization current is DC 18.0A~20.0A. At the end of the melting process, 50kg~100kg of electrodes are reserved for arc extinguishing. During arc extinguishing, the melting current is required to decrease by 1KA per minute, the voltage by 1V, and the arc stabilization current by 1A, for a total of four times, until the melting process ends. The entire arc extinguishing process takes 4min~6min. At the same time, during arc extinguishing, the arc stabilization current is changed from DC to AC, and the stirring cycle is 15s~30s.

[0041] Step 3: Primary Ingot Processing

[0042] The flash at the head of the primary ingot prepared in step two is removed by machine.

[0043] Step 4: Secondary or tertiary smelting

[0044] The primary ingot obtained after step three is used as a consumable electrode in a vacuum consumable arc furnace for secondary melting to obtain a secondary ingot. When loading the furnace, the primary ingot must be inverted, i.e., head down. If a third melting is to be performed, the secondary ingot is loaded into the furnace with its head inverted.

[0045] Specifically, the parameters set for the secondary melting are as follows: melting current is 18.0KA~28.0KA, melting voltage is 29.0V~40.0V, arc stabilization current is AC 10.0A~25.0A, and stirring cycle is 15s~60s.

[0046] The parameters set for the three melting processes are as follows: melting current of 20.0KA~28.0KA, melting voltage of 30.0V~40.0V, arc stabilization current of AC 15.0A~25.0A, and stirring cycle of 15s~60s.

[0047] Step 5: Processing, Sampling and Analysis

[0048] The titanium alloy ingot obtained from the final melting in step four is processed to the target size, and samples are taken for analysis. If the analysis results meet the requirements of GB / T3620.1 standard and the composition is uniform, the finished titanium alloy ingot is qualified; otherwise, it is unqualified.

[0049] To further verify the effectiveness of the preparation method of the present invention, the inventors conducted the following specific experiments:

[0050] Example 1 (Preparation of TC4 titanium alloy ingot with a diameter of Φ630mm)

[0051] In this embodiment, TC4 titanium alloy (nominal composition Ti-6Al-4V) is prepared by a three-stage melting method. The specific preparation process is as follows:

[0052] 1) Weigh out the sponge titanium, aluminum vanadium master alloy, aluminum granules and titanium dioxide according to the mass percentage, mix them evenly and then press them into electrode blocks, and then weld the pressed electrode blocks into electrodes.

[0053] 2) The electrode obtained in step 1) is used as a consumable electrode and smelted in a vacuum consumable arc furnace to finally obtain a Φ500mm primary ingot, such as... Figure 2 As shown. The specific parameters for a single melting operation are as follows: melting current is 16.0 kA, melting voltage is 33.0 V, and arc stabilization current is DC 18.0 A; the weight reserved for arc termination is 50 kg; during arc termination, the melting current decreases by 1 kA per minute, i.e.: 16.0 → 15.0 → 14.0 → 13.0; the melting voltage decreases by 1 V per minute, i.e.: 33.0 → 32.0 → 31.0 → 30.0; the arc stabilization current decreases by 1 A per minute, i.e.: AC18.0 → AC17.0 → AC16.0 → AC15.0; the stirring cycle is 15 s; and the total arc termination time is 4 min.

[0054] 3) After measurement, the flash thickness of the first ingot is 15mm. The first ingot is processed to remove the flash at the head. The processing amount per piece is about 2kg.

[0055] 4) The primary ingot obtained after processing in step 3) is used as a consumable electrode in a vacuum consumable arc furnace for secondary melting to obtain a Φ560mm secondary ingot. When loading the furnace, the primary ingot must be inverted, i.e., head down. The specific parameters for secondary melting are as follows: melting current is 18.0KA~24.0KA, melting voltage is 29.0V~36.0V, arc stabilization current is AC 10.0A~20.0A, and stirring cycle is 15s~60s.

[0056] 5) The secondary ingot obtained in step 4) is used as a consumable electrode and smelted three times in a vacuum consumable arc furnace to obtain a Φ630mm tertiary ingot. When loading the furnace, the head of the secondary ingot must be inverted. The specific parameters for the three smelting processes are as follows: smelting current is 20.0KA~25.0KA, smelting voltage is 30.0V~40.0V, arc stabilization current is AC 15.0A~25.0A, and stirring cycle is 15s~60s.

[0057] 6) Samples were taken from the head, middle, and tail sections of the Φ630mm ternary ingot obtained in step 5) for analysis. The chemical composition test results are shown in Table 1 below:

[0058] Table 1 Chemical composition of ingots

[0059]

[0060] As can be seen from the comparison of the data in Table 1 with GB / T3620.1, the composition of the TC4 titanium alloy ingot with a specification of Φ630mm prepared in Example 1 of the present invention meets the requirements of GB / T3620.1 standard, and the composition has good uniformity.

[0061] Example 2 (Preparation of TC4 titanium alloy ingot with a diameter of Φ720mm)

[0062] In this embodiment, TC4 titanium alloy (nominal composition Ti-6Al-4V) is prepared by a three-stage melting method. The specific preparation process is as follows:

[0063] 1) Weigh out the sponge titanium, aluminum vanadium master alloy, aluminum granules and titanium dioxide according to the mass percentage, mix them evenly and then press them into electrode blocks, and then weld the pressed electrode blocks into electrodes.

[0064] 2) The electrode obtained in step 1) is used as a consumable electrode and smelted in a vacuum consumable arc furnace to finally obtain a Φ540mm primary ingot. The specific parameters for the primary smelting are set as follows: smelting current is 18.0KA, smelting voltage is 34.0V, and arc stabilization current is DC 18.0A; the weight reserved for arc termination is 60kg; during arc termination, the smelting current decreases by 1KA per minute, i.e.: 18.0→17.0→16.0→15.0; the smelting voltage decreases by 1V per minute, i.e.: 34.0→33.0→32.0→31.0; the arc stabilization current decreases by 1A per minute, i.e. AC18.0→AC17.0→AC16.0→AC15.0; the stirring cycle is 20s; and the total arc termination time is 4min.

[0065] 3) After measurement, the flash thickness of the first ingot is 16mm. The first ingot is processed to remove the flash at the head. The processing amount per piece is about 2kg.

[0066] 4) The primary ingot obtained after processing in step 3) is used as a consumable electrode in a vacuum consumable arc furnace for secondary melting to obtain a Φ630mm secondary ingot. When loading the furnace, the primary ingot must be inverted, i.e., head down. The specific parameters for secondary melting are as follows: melting current is 20.0KA~25.0KA, melting voltage is 30.0V~38.0V, arc stabilization current is AC 10.0A~20.0A, and stirring cycle is 15s~60s.

[0067] 5) The secondary ingot obtained in step 4) is used as a consumable electrode and smelted three times in a vacuum consumable arc furnace to obtain a Φ720mm tertiary ingot. When loading the furnace, the head of the secondary ingot must be inverted. The specific parameters for the three smelting are as follows: smelting current is 22.0KA~28.0KA, smelting voltage is 30.0V~40.0V, arc stabilization current is AC 15.0A~25.0A, and stirring cycle is 15s~60s.

[0068] 6) Samples were taken from the head, middle, and tail sections of the Φ720mm ternary ingot obtained in step 5) for analysis. The chemical composition test results are shown in Table 2 below:

[0069] Table 2 Chemical composition of ingots

[0070]

[0071] As can be seen from the comparison of the data in Table 2 with GB / T3620.1, the composition of the TC4 titanium alloy ingot with a specification of Φ720mm prepared in Example 2 of the present invention meets the requirements of GB / T3620.1 standard, and the composition has good uniformity.

[0072] Example 3 (Preparation of TC4 titanium alloy ingot with a diameter of Φ640mm)

[0073] In this embodiment, TC4 titanium alloy (nominal composition Ti-6Al-4V) is prepared by a two-stage melting method. The specific preparation process is as follows:

[0074] 1) Weigh out the sponge titanium, aluminum vanadium master alloy, aluminum granules and titanium dioxide according to the mass percentage, mix them evenly and then press them into electrode blocks, and then weld the pressed electrode blocks into electrodes.

[0075] 2) The electrode obtained in step 1) is used as a consumable electrode and smelted in a vacuum consumable arc furnace to finally obtain a Φ570mm primary ingot. The specific parameters for the primary smelting are set as follows: smelting current is 20.0KA, smelting voltage is 35.0V, and arc stabilization current is DC 19.0A; the weight reserved for arc termination is 80kg. During arc termination, the smelting current decreases by 1KA per minute, i.e., 20.0→19.0→18.0→17.0, the smelting voltage decreases by 1V per minute, i.e., 35.0→34.0→33.0→32.0, and the arc stabilization current decreases by 1A per minute, i.e., AC19.0→AC18.0→AC17.0→AC16.0. The stirring cycle is 30s, and the total arc termination time is 5min.

[0076] 3) After measurement, the flash thickness of the first ingot is 14mm. The first ingot is processed to remove the flash at the head. The processing amount per piece is about 2.5kg.

[0077] 4) The primary ingot obtained after processing in step 3) is used as a consumable electrode in a vacuum consumable arc furnace for secondary melting to obtain a Φ640mm secondary ingot. When loading the furnace, the primary ingot must be inverted, i.e., head down. The specific parameters for secondary melting are as follows: melting current is 20.0KA~25.0KA, melting voltage is 30.0V~38.0V, arc stabilization current is AC 10.0A~20.0A, and stirring cycle is 15s~60s.

[0078] 5) Samples were taken from the head, middle, and tail sections of the Φ640mm ingot obtained in step 4) for analysis. The chemical composition test results are shown in Table 3 below:

[0079] Table 3 Chemical composition of ingots

[0080]

[0081] As can be seen from the comparison of the data in Table 3 with GB / T3620.1, the composition of the TC4 titanium alloy ingot with a specification of Φ640mm prepared in Example 3 of the present invention meets the requirements of GB / T3620.1 standard, and the composition has good uniformity.

[0082] Example 4 (Preparation of TA15 titanium alloy ingot with a diameter of Φ720mm)

[0083] In this embodiment, TA15 titanium alloy (nominal composition Ti-6.5Al-1Mo-1V-2Zr) is prepared using a three-stage melting method. The specific preparation process is as follows:

[0084] 1) Weigh out the sponge titanium, aluminum vanadium master alloy, aluminum molybdenum master alloy, aluminum granules, sponge zirconium, and titanium dioxide according to the mass percentage, mix them evenly, press them into electrode blocks, and then weld the pressed electrode blocks into electrodes.

[0085] 2) The electrode obtained in step 1) is used as a consumable electrode and smelted in a vacuum consumable arc furnace to finally obtain a Φ570mm primary ingot. The specific parameters for the primary smelting are set as follows: smelting current is 21.0KA, smelting voltage is 35.0V, and arc stabilization current is DC 19.0A; the weight reserved for arc termination is 80kg. During arc termination, the smelting current decreases by 1KA per minute, 21.0→20.0→19.0→18.0, the smelting voltage decreases by 1V per minute, i.e., 35.0→34.0→33.0→32.0, and the arc stabilization current decreases by 1A per minute, i.e., AC19.0→AC18.0→AC17.0→AC16.0. The stirring cycle is 30s, and the total arc termination time is 5min.

[0086] 3) After measurement, the flash thickness of the first ingot is 10mm. The first ingot is processed to remove the flash at the head. The processing amount per piece is about 1.5kg.

[0087] 4) The primary ingot obtained after processing in step 3) is used as a consumable electrode in a vacuum consumable arc furnace for secondary melting to obtain a Φ630mm secondary ingot. When loading the furnace, the primary ingot must be inverted, i.e., head down. The specific parameters for secondary melting are as follows: melting current is 20.0KA~25.0KA, melting voltage is 30.0V~38.0V, arc stabilization current is AC 10.0A~20.0A, and stirring cycle is 15s~60s.

[0088] 5) The secondary ingot obtained in step 4) is used as a consumable electrode and smelted three times in a vacuum consumable arc furnace to obtain a Φ720mm tertiary ingot. When loading the furnace, the head of the secondary ingot must be inverted. The specific parameters for the three smelting are as follows: smelting current is 22.0KA~28.0KA, smelting voltage is 30.0V~40.0V, arc stabilization current is AC 15.0A~25.0A, and stirring cycle is 15s~60s.

[0089] 6) Samples were taken from the head, middle, and tail sections of the Φ720mm ternary ingot obtained in step 5) for analysis. The chemical composition test results are shown in Table 4 below:

[0090] Table 4 Chemical composition of ingots

[0091]

[0092] As can be seen from the comparison of the data in Table 4 with GB / T3620.1, the composition of the TA15 titanium alloy ingot with a specification of Φ720mm prepared in Example 4 of the present invention meets the requirements of GB / T3620.1 standard, and the composition has good uniformity.

[0093] Example 5 (Preparation of TC4 titanium alloy ingot with a diameter of Φ720mm)

[0094] In this embodiment, TC4 titanium alloy (nominal composition Ti-6Al-4V) is prepared by a two-stage melting method. The specific preparation process is as follows:

[0095] 1) Weigh out the sponge titanium, aluminum vanadium master alloy, aluminum granules and titanium dioxide according to the mass percentage, mix them evenly and then press them into electrode blocks, and then weld the pressed electrode blocks into electrodes.

[0096] 2) The electrode obtained in step 1) is used as a consumable electrode and smelted in a vacuum consumable arc furnace to finally obtain a Φ640mm primary ingot. The specific parameters for the primary smelting are set as follows: smelting current is 22.0KA, smelting voltage is 36.0V, and arc stabilization current is DC 20.0A; the weight reserved for arc termination is 100kg. During arc termination, the smelting current decreases by 1KA per minute, i.e.: 22.0→21.0→20.0→19.0, the smelting voltage decreases by 1V per minute, i.e.: 36.0→35.0→34.0→33.0, and the arc stabilization current decreases by 1A per minute, i.e. AC20.0→AC19.0→AC18.0→AC17.0. The stirring cycle is 30s, and the total arc termination time is 6min.

[0097] 3) After measurement, the flash thickness of the first ingot is 20mm. The first ingot is processed to remove the flash at the head. The processing amount per piece is about 3kg.

[0098] 4) The primary ingot processed in step 3) is used as a consumable electrode in a vacuum consumable arc furnace for secondary melting to obtain a Φ720mm secondary ingot. When loading the furnace, the primary ingot must be inverted, i.e., head down. The specific parameters for secondary melting are as follows: melting current is 22.0KA~28.0KA, melting voltage is 30.0V~40.0V, arc stabilization current is AC 15.0A~25.0A, and stirring cycle is 15s~60s.

[0099] 5) Samples were taken from the head, middle, and tail sections of the Φ720mm ingots obtained in step 4) for analysis. The chemical composition test results are shown in Table 5 below:

[0100] Table 5 Chemical composition of ingots

[0101]

[0102] As can be seen from the comparison of the data in Table 5 with GB / T3620.1, the composition of the TC4 titanium alloy ingot with a specification of Φ720mm prepared in Example 5 of the present invention meets the requirements of GB / T3620.1 standard, and the composition has good uniformity.

[0103] In summary, the VAR melting method employed in this invention strictly controls the specific parameters of each melting process. In particular, by adjusting the melting current, voltage, and arc-stabilizing current four times during the final arc termination stage of a single melting process, the depth of the molten pool is reduced, stirring is weakened, and flash height is decreased. Simultaneously, the reduced voltage shortens the arc and weakens the arc-climbing phenomenon, ensuring safe and stable melting. Furthermore, the use of AC for arc stabilization during arc termination ensures thorough stirring of the molten pool, improving the situation where the molten pool does not reach the edge, and avoiding the arc deviation problem caused by DC stirring. Ultimately, this reduces the problem of excessively thick flash at the head of commonly used industrial ingots of Φ500mm to Φ640mm, reducing processing volume and significantly improving the production efficiency and yield of the target titanium alloy ingots. Moreover, the final titanium alloy ingot composition meets the requirements of GB / T3620.1 standard and is uniformly consistent.

[0104] The above description is merely a specific embodiment of the present invention, enabling those skilled in the art to understand or implement the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention.

[0105] It should be understood that the present invention is not limited to the content already described above, and various modifications and changes can be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A smelting method for improving the production efficiency and yield of titanium alloy ingots, characterized in that, Includes the following steps: Step 1: Electrode Preparation The constituent raw materials are determined according to the chemical composition of the target titanium alloy ingot. Then, each constituent raw material is weighed according to the mass percentage and mixed evenly before being pressed into electrode blocks. Then, several electrode blocks are welded together to form an electrode. Step 2: First Melting The electrode obtained in step one is used as a consumable electrode. Under set parameters, the consumable electrode is melted once in a vacuum consumable arc furnace to finally obtain a primary ingot. Step 3: Primary Ingot Processing The flash at the head of the primary ingot prepared in step two is removed by machine. Step 4: Secondary or tertiary smelting The primary ingot obtained after step three is used as a consumable electrode and then remelted in a vacuum consumable arc furnace to obtain a secondary ingot. When loading the furnace, the primary ingot must be inverted, i.e., head down. If a third remelting is to be performed, the secondary ingot is loaded into the furnace with its head upside down. Step 5: Processing, Sampling and Analysis The titanium alloy ingot obtained from the final melting in step four is processed to the target size, and the ingot is sampled and analyzed. If the analysis results meet the requirements of GB / T3620.1 standard and the composition is uniform, the titanium alloy finished ingot is qualified; otherwise, it is unqualified. The parameters set during the first melting in step two are as follows: melting current is 16.0kA~22.0kA, melting voltage is 33.0V~36.0V, arc stabilization current is DC 18.0A~20.0A, and 50kg~100kg of electrode is reserved at the end of melting for arc extinguishing; In step two, during the arc extinguishing of a single melting process, the melting current is required to decrease by 1kA, the voltage by 1V, and the arc stabilizing current by 1A per minute, for a total of four times, until the melting is completed. In step two, during the initial melting and arc termination, the arc stabilizing current is changed from DC to AC, and the stirring cycle is 15s to 30s.

2. The smelting method for improving the production efficiency and yield of titanium alloy ingots according to claim 1, characterized in that, In step two, during the initial melting and arc extinguishing, the entire arc extinguishing process takes 4 to 6 minutes.

3. The smelting method for improving the production efficiency and yield of titanium alloy ingots according to claim 1, characterized in that, The thickness of the flash of the ingot obtained after one melting in step two is within 20mm.

4. The smelting method for improving the production efficiency and yield of titanium alloy ingots according to claim 1, characterized in that, The parameters set for the secondary melting in step four are as follows: melting current is 18.0kA~28.0kA, melting voltage is 29.0V~40.0V, arc stabilization current is AC 10.0A~25.0A, and stirring cycle is 15s~60s.

5. The smelting method for improving the production efficiency and yield of titanium alloy ingots according to claim 1, characterized in that, The parameters set for the three melting processes in step four are as follows: melting current is 20.0kA~28.0kA, melting voltage is 30.0V~40.0V, arc stabilization current is AC 15.0A~25.0A, and stirring cycle is 15s~60s.

6. The smelting method for improving the production efficiency and yield of titanium alloy ingots according to any one of claims 1 to 5, characterized in that, The smelting method is used to prepare titanium alloy primary ingots with dimensions of Φ500mm to Φ640mm.

Citation Information

Patent Citations

  • Smelting and feeding method for titanium alloy ingots with common industrial specification

    CN110669955A

  • Arc extinguishing process of VAR titanium alloy primary ingot

    CN110964932A