A high-temperature titanium alloy material with high strength and high toughness and a preparation method thereof

High-temperature titanium alloys were prepared by using the Ti-Al-Nb-Mo-Sn-Zr-Si-O alloy system and a specific process, which solved the problem of insufficient strength and plasticity matching of traditional high-temperature titanium alloys at high temperatures, and achieved comprehensive mechanical properties of high strength and high toughness at 600℃.

CN117535555BActive Publication Date: 2026-11-24XIAN SUPERCRYSYAL SCI TECH DEV CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311414224.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-30
Publication Date
2026-11-24
Estimated Expiration
2043-10-30

AI Technical Summary

Technical Problem

Traditional high-temperature titanium alloys have poor thermal strength and thermal stability when the service temperature exceeds 600℃, making it difficult to strengthen them through heat treatment. The high-temperature strength and plasticity are not well matched.

Method used

High-strength and high-toughness high-temperature titanium alloy materials were prepared by using the Ti-Al-Nb-Mo-Sn-Zr-Si-O alloy system through vacuum consumable arc melting, free forging and heat treatment processes.

Benefits of technology

At room temperature and 600°C, the alloy material exhibits high strength and high toughness, with significantly improved tensile strength, yield strength, elongation and reduction of area, meeting the high-temperature service requirements of aerospace engines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117535555B_ABST
    Figure CN117535555B_ABST
Patent Text Reader

Abstract

The application relates to a high-temperature titanium alloy material with high strength and high toughness and a preparation method thereof. The titanium alloy material system comprises the following components in percentage by mass: Al: 5.8-7.2%, Nb: 0.5-2%, Mo: 1.0-3.0%, Sn: 0.9-1.5%, Zr: 1.5-3.5%, Si: 0.2-0.5%, O: 0.05-0.25%, and the balance of Ti. The preparation method comprises electrode preparation, vacuum consumable arc smelting, free forging and heat treatment. The titanium alloy material prepared by the application has excellent strength and toughness at room temperature and 600 DEG C, and has good strength and toughness matching at room temperature and 600 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of titanium alloy technology, and in particular to a high-temperature titanium alloy material with high thermal strength and toughness and its preparation method. Technical Background

[0002] Titanium alloys possess excellent properties such as low density, high specific strength, and good corrosion resistance, making them widely used in high-performance structural components for aerospace engines. However, with the continuous improvement of the thrust-to-weight ratio of aero-engines, the requirements for the service temperature of engine structural components are becoming increasingly stringent. Currently, the maximum service temperature of high-temperature titanium alloys does not exceed 600℃. Traditional high-temperature titanium alloys are generally near-α type titanium alloys, with mature and typical alloys including IMI834, BT25, Ti60, and Ti1100. However, when the service temperature exceeds 600℃, the thermal strength or thermal stability of traditional high-temperature titanium alloys deteriorates. These traditional near-α type titanium alloys, due to their low β-stabilizing element content, mainly rely on the solid solution precipitation strengthening of the α phase and the precipitation strengthening effect of silicides produced by the addition of Si to improve high-temperature creep performance and thermal stability. The low β-stabilizing element content also makes it difficult to strengthen them through heat treatment, thus their high-temperature strength cannot be significantly improved. To improve the service temperature of high-temperature titanium alloys, a good match between high-temperature strength and high-temperature plasticity has always been the key to research on high-temperature titanium alloys. Summary of the Invention

[0003] To address the shortcomings of existing technologies, this invention provides a high-temperature titanium alloy material with high thermal strength and high toughness through element alloying, exhibiting comprehensive mechanical properties of high strength and high toughness at both room temperature and 600℃.

[0004] This invention also proposes a method for preparing high-temperature titanium alloy materials with high thermal strength and high toughness. Through vacuum consumable arc melting, free forging and heat treatment, a high-temperature titanium alloy material with high strength and high toughness comprehensive mechanical properties at room temperature and 600℃ is prepared.

[0005] To achieve the above objectives, the present invention adopts the following technical solution:

[0006] A high-temperature titanium alloy material with high thermal strength and high toughness, the system being Ti-Al-Nb-Mo-Sn-Zr-Si-O;

[0007] Preferably, the system comprises, by mass percentage: Al: 5.8%–7.2%, Nb: 0.5%–2%, Mo: 1.0%–3.0%, Sn: 0.9%–1.5%, Zr: 1.5%–3.5%, Si: 0.2%–0.5%, O: 0.05%–0.25%, with the balance being Ti.

[0008] A method for preparing a high-temperature titanium alloy material with high thermal strength and toughness, characterized by comprising the following steps:

[0009] S1. Calculate the amount of raw materials according to the mass percentage of the high-temperature titanium alloy material system with high thermal strength and high toughness designed, weigh the raw materials according to the calculation results, mix the weighed raw materials and press them into electrode blocks by hydraulic press, and then weld them into consumable electrodes by vacuum plasma welding.

[0010] S2. The consumable electrode is melted into an ingot by vacuum consumable arc melting;

[0011] S3. The ingot prepared in S2 is forged into a forging blank, and the forging blank is air-cooled.

[0012] S4. Heat treat the forged billet after air cooling in S3.

[0013] Preferably, the raw materials are: sponge titanium, aluminum-molybdenum alloy, aluminum-niobium alloy, aluminum briquettes, titanium-tin alloy, sponge zirconium, titanium-silicon alloy, and titanium dioxide.

[0014] Preferably, the hydraulic press in S1 has a pressing pressure of 20-25 MPa and a holding time of 20-25 seconds.

[0015] Preferably, vacuum consumable arc melting in S2 is performed three times.

[0016] Preferably, in the three-stage vacuum arc melting process, the vacuum degree of the first vacuum arc melting is ≤1.0×10⁻¹ Pa, the melting current is 5–7 kA, the melting voltage is 25–35 V, and the arc stabilizing current is DC 5 A; the vacuum degree of the second vacuum arc melting is ≤1.0×10⁻¹ Pa, the melting current is 6–8 kA, the melting voltage is 23–30 V, and the arc stabilizing current is AC 6 A / 30 s; the vacuum degree of the third vacuum arc melting is ≤1.0×10⁻¹ Pa, the melting current is 7–9 kA, the melting voltage is 25–35 V, and the arc stabilizing current is AC 7 A / 30 s.

[0017] Preferably, the free forging process in S3 consists of six heating cycles, two upsetting cycles, and two drawing cycles. The temperatures of the six heating cycles are 1150℃, 960℃, 920℃, 920℃, 910℃, and 910℃, respectively, and the upsetting deformation amount for each heating cycle is 50-60%.

[0018] Preferably, the heat treatment method described in S4 is as follows: after solution heat treatment, water cooling is performed, followed by aging heat treatment, and then air cooling is performed.

[0019] Preferably, the solution heat treatment temperature is T. β -20~40℃, heat treatment time is 2~4h, and the aging heat treatment temperature is 500~600℃ for 4~8h.

[0020] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0021] (1) This invention designs a Ti-Al-Nb-Mo-Sn-Zr-Si-O alloy through alloying, which has a good match between high-temperature strength and high-temperature plasticity;

[0022] (2) The present invention enables the alloy to have high strength and high toughness comprehensive mechanical properties at room temperature and 600℃ after three vacuum self-consuming arc melting, six-fire two-upsetting two-drawing free forging and solution aging heat treatment. Attached Figure Description

[0023] Figure 1 This is a schematic diagram of the solid solution aged microstructure of the high-temperature titanium alloy with high thermal strength and toughness in Example 1 of the present invention. Specific Implementation

[0024] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0025] Example 1

[0026] A high-temperature titanium alloy material with high thermal strength and toughness has a system of Ti-Al-Nb-Mo-Sn-Zr-Si-O. The elements in the system are designed by mass percentage as follows: Al: 7.2%, Nb: 2%, Mo: 3.0%, Sn: 1.5%, Zr: 3.5%, Si: 0.5%, O: 0.25%, with the balance being Ti. The preparation method is as follows:

[0027] S1, Electrode Preparation

[0028] The amounts of raw materials sponge titanium, aluminum-molybdenum alloy, aluminum-niobium alloy, aluminum briquettes, titanium-tin alloy, sponge zirconium, titanium-silicon alloy, and titanium dioxide were calculated based on the mass percentage of the element composition in the designed high-temperature titanium alloy material system with high thermal strength and high toughness. The raw materials were weighed according to the calculation results, mixed, and pressed into electrode blocks by a hydraulic press at a pressure of 25 MPa and a holding time of 20 s. The blocks were then vacuum plasma welded into consumable electrodes.

[0029] S2, Vacuum self-consuming arc melting

[0030] The consumable electrode prepared in S1 was then cast into an ingot through three vacuum consumable arc melting processes, wherein the vacuum degree of the first vacuum consumable arc melting process was 1.0 × 10⁻⁶. -1 Pa, melting current 7KA, melting voltage 35V, arc stabilizing current DC 5A, vacuum degree of the second vacuum self-consuming arc melting 1.0×10-1 The melting current is 8 kA, the melting voltage is 30 V, the arc stabilization current is AC 6 A / 30 s, and the vacuum degree of the third vacuum self-consuming arc melting is 1.0 × 10⁻⁶ Pa. -1 Pa, melting current is 9KA, melting voltage is 35V, and arc stabilization current is AC 7A / 30s;

[0031] S3, Free Forging

[0032] The ingot prepared in S2 was forged into a forging billet by six forging cycles of two upsetting and two drawing. The forging billet was then air-cooled. The forging temperatures of the six forging cycles were 1150℃, 960℃, 920℃, 920℃, 910℃, and 910℃, respectively. The upsetting deformation amount of each forging cycle was 60%.

[0033] S4, Heat Treatment

[0034] After air cooling, the forged billet of S3 undergoes solution heat treatment, followed by water cooling, aging heat treatment, and then air cooling. The solution heat treatment is carried out at T... β The forging billet was held at -20℃ for 2 hours, followed by aging heat treatment at 600℃ for 4 hours. A schematic diagram of the solution-aged microstructure of the forging billet after heat treatment is shown below. Figure 1 As shown.

[0035] The mechanical properties of the titanium alloy material prepared in Example 1 at room temperature and 600℃ are shown in Table 1.

[0036] Table 1 Mechanical properties of the alloy prepared in Example 1

[0037]

[0038] Example 2

[0039] A high-temperature titanium alloy material with high thermal strength and toughness has a system of Ti-Al-Nb-Mo-Sn-Zr-Si-O. The elements in the system are designed by mass percentage as follows: Al: 5.8%, Nb: 0.5%, Mo: 1.0%, Sn: 0.9%, Zr: 1.5%, Si: 0.2%, O: 0.05%, with the balance being Ti. The preparation method is as follows:

[0040] S1, Electrode Preparation

[0041] The amounts of raw materials, including sponge titanium, aluminum-molybdenum alloy, aluminum-niobium alloy, aluminum briquettes, titanium-tin alloy, sponge zirconium, titanium-silicon alloy, and titanium dioxide, were calculated based on the mass percentage of the elements in the designed high-temperature titanium alloy material system with high thermal strength and toughness. The raw materials were weighed according to the calculation results, mixed, and pressed into electrode blocks by a hydraulic press at a pressure of 20 MPa and a holding time of 25 s. The blocks were then vacuum plasma welded into consumable electrodes.

[0042] S2, Vacuum self-consuming arc melting

[0043] The consumable electrode prepared in S1 was then cast into an ingot through three vacuum consumable arc melting processes, wherein the vacuum degree of the first vacuum consumable arc melting process was 0.9 × 10⁻⁶. -1 Pa, melting current 5KA, melting voltage 25V, arc stabilizing current DC 5A, vacuum degree of the second vacuum self-consuming arc melting is 1.0×10 -1 The melting current was 6 kA, the melting voltage was 23 V, the arc stabilization current was AC 6 A / 30 s, and the vacuum degree of the third vacuum self-consuming arc melting was 0.8 × 10⁻⁶ Pa. -1 Pa, melting current is 7KA, melting voltage is 25V, and arc stabilization current is AC 7A / 30s;

[0044] S3, Free Forging

[0045] The ingot prepared in S2 was forged into a forging billet by six forging cycles of two upsetting and two drawing. The forging billet was then air-cooled. The forging temperatures of the six forging cycles were 1150℃, 960℃, 920℃, 920℃, 910℃, and 910℃, respectively. The upsetting deformation amount of each forging cycle was 50%.

[0046] S4, Heat Treatment

[0047] After air cooling, the forged billet of S3 undergoes solution heat treatment, followed by water cooling, aging heat treatment, and then air cooling. The solution heat treatment is carried out at T... β After holding at -40℃ for 4 hours, the aging heat treatment is carried out by holding at 500℃ for 8 hours.

[0048] The mechanical properties of the titanium alloy material prepared in Example 2 at room temperature and 600℃ are shown in Table 2.

[0049] Table 2 Mechanical properties of the alloy prepared in Example 2

[0050]

[0051] Example 3:

[0052] A high-temperature titanium alloy material with high thermal strength and toughness has a system of Ti-Al-Nb-Mo-Sn-Zr-Si-O. The elements in the system are designed by mass percentage as follows: Al: 6.3%, Nb: 1.5%, Mo: 1.5%, Sn: 1.4%, Zr: 2.0%, Si: 0.4%, O: 0.1%, with the balance being Ti. The preparation method is as follows:

[0053] S1, Electrode Preparation

[0054] The amounts of raw materials sponge titanium, aluminum-molybdenum alloy, aluminum-niobium alloy, aluminum briquettes, titanium-tin alloy, sponge zirconium, titanium-silicon alloy, and titanium dioxide were calculated based on the mass percentage of the element composition in the designed high-temperature titanium alloy material system with high thermal strength and high toughness. The raw materials were weighed according to the calculation results, mixed, and pressed into electrode blocks by a hydraulic press at a pressure of 22 MPa and a holding time of 23 s. The blocks were then vacuum plasma welded into consumable electrodes.

[0055] S2, Vacuum self-consuming arc melting

[0056] The consumable electrode prepared in S1 was then cast into an ingot through three vacuum consumable arc melting processes, wherein the vacuum degree of the first vacuum consumable arc melting process was 1.0 × 10⁻⁶. -1 Pa, melting current 6KA, melting voltage 30V, arc stabilization current DC 5A, vacuum degree of the second vacuum self-consuming arc melting 0.8×10 -1 The melting current was 7 kA, the melting voltage was 27 V, the arc stabilization current was AC 6 A / 30 s, and the vacuum degree of the third vacuum self-consuming arc melting was 0.9 × 10⁻⁶ Pa. -1 Pa, melting current is 8KA, melting voltage is 30V, and arc stabilization current is AC 7A / 30s;

[0057] S3, Free Forging

[0058] The ingot prepared in S2 was forged into a forging billet by six forging cycles of two upsetting and two drawing. The forging billet was then air-cooled. The forging temperatures of the six forging cycles were 1150℃, 960℃, 920℃, 920℃, 910℃, and 910℃, respectively. The upsetting deformation amount of each forging cycle was 53%.

[0059] S4, Heat Treatment

[0060] After air cooling, the forged billet of S3 undergoes solution heat treatment, followed by water cooling, aging heat treatment, and then air cooling. The solution heat treatment is carried out at T... β After holding at -25℃ for 3 hours, the aging heat treatment is carried out by holding at 550℃ for 6 hours.

[0061] The mechanical properties of the titanium alloy material prepared in Example 3 at room temperature and 600℃ are shown in Table 3.

[0062] Table 3 Mechanical properties of the alloy prepared in Example 3

[0063]

[0064] Example 4:

[0065] A high-temperature titanium alloy material with high thermal strength and toughness has a system of Ti-Al-Nb-Mo-Sn-Zr-Si-O. The elements in the system are designed by mass percentage as follows: Al: 6.8%, Nb: 1.0%, Mo: 2.5%, Sn: 1.2%, Zr: 3.0%, Si: 0.3%, O: 0.2%, with the balance being Ti. The preparation method is as follows:

[0066] S1, Electrode Preparation

[0067] The amounts of raw materials, including sponge titanium, aluminum-molybdenum alloy, aluminum-niobium alloy, aluminum briquettes, titanium-tin alloy, sponge zirconium, titanium-silicon alloy, and titanium dioxide, were calculated based on the mass percentage of the elements in the designed high-temperature titanium alloy material system with high thermal strength and toughness. The raw materials were weighed according to the calculation results, mixed, and pressed into electrode blocks by a hydraulic press at a pressure of 23 MPa and a holding time of 22 s. The blocks were then vacuum plasma welded into consumable electrodes.

[0068] S2, Vacuum self-consuming arc melting

[0069] The consumable electrode prepared in S1 was then cast into an ingot through three vacuum consumable arc melting processes, wherein the vacuum degree of the first vacuum consumable arc melting process was 0.8 × 10⁻⁶. -1 The melting current is 7 kA, the melting voltage is 30 V, the arc stabilizing current is DC 5 A, and the vacuum degree of the second vacuum self-consuming arc melting is 0.9 × 10⁻⁶ Pa. -1 The melting current was 8 kA, the melting voltage was 28 V, the arc stabilization current was AC 6 A / 30 s, and the vacuum degree of the third vacuum self-consuming arc melting was 0.9 × 10⁻⁶ Pa. -1 Pa, melting current is 9KA, melting voltage is 33V, and arc stabilization current is AC 7A / 30s;

[0070] S3, Free Forging

[0071] The ingot prepared in S2 was forged into a forging billet by six forging cycles of two upsetting and two drawing. The forging billet was then air-cooled. The forging temperatures of the six forging cycles were 1150℃, 960℃, 920℃, 920℃, 910℃, and 910℃, respectively. The upsetting deformation amount of each forging cycle was 57%.

[0072] S4, Heat Treatment

[0073] After air cooling, the forged billet of S3 undergoes solution heat treatment, followed by water cooling, aging heat treatment, and then air cooling. The solution heat treatment is carried out at T... β After holding at -30℃ for 3 hours, the aging heat treatment is carried out by holding at 580℃ for 5 hours.

[0074] The mechanical properties of the titanium alloy material prepared in Example 4 at room temperature and 600℃ are shown in Table 4.

[0075] Table 4 Mechanical properties of the alloy prepared in Example 4

[0076]

[0077] As can be seen from Tables 1 to 4, the titanium alloy prepared by this invention has a tensile strength ≥1200MPa, a yield strength ≥1050MPa, an elongation ≥12%, and a reduction of area ≥40% at room temperature. At 600℃, the tensile strength ≥720MPa, the yield strength ≥550MPa, the elongation ≥20%, and the reduction of area ≥75%. Compared with the prior art, the tensile strength is increased by more than 6%, the yield strength by more than 2%, the elongation by more than 10%, and the reduction of area by more than 15%.

[0078] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claimed invention.

Claims

1. A method for preparing a high-temperature titanium alloy material with high thermal strength and high toughness, characterized in that, Includes the following steps: S1. Calculate the amount of raw materials according to the mass percentage of the high-temperature titanium alloy material system with high thermal strength and high toughness designed, weigh the raw materials according to the calculation results, mix the weighed raw materials and press them into electrode blocks by hydraulic press, and then weld them into consumable electrodes by vacuum plasma welding. S2. The consumable electrode is melted into an ingot by vacuum consumable arc melting; S3. After the ingot prepared in S2 is forged into a forging billet through six heating cycles, two upsetting cycles, and two drawing cycles, the forging billet is air-cooled. The temperatures of the six heating cycles are 1150℃, 960℃, 920℃, 920℃, 910℃, and 910℃ respectively, and the upsetting deformation amount of each heating cycle is 50~60%. S4. Heat-treat the forging billet after air cooling in S3. The heat treatment method is as follows: after solution heat treatment, water cooling is performed, followed by aging heat treatment, and then air cooling is performed. The high-temperature titanium alloy material system is Ti-Al-Nb-Mo-Sn-Zr-Si-O, and the system comprises the following mass percentages: Al: 5.8%~7.2%, Nb: 0.5%~2%, Mo: 1.0%~3.0%, Sn: 0.9%~1.5%, Zr: 1.5%~3.5%, Si: 0.2%~0.5%, O: 0.05%~0.25%, with the balance being Ti.

2. The method for preparing a high-temperature titanium alloy material with high thermal strength and toughness according to claim 1, characterized in that, The raw materials are: sponge titanium, aluminum-molybdenum alloy, aluminum-niobium alloy, aluminum briquettes, titanium-tin alloy, sponge zirconium, titanium-silicon alloy, and titanium dioxide.

3. The method for preparing a high-temperature titanium alloy material with high thermal strength and toughness according to claim 1, characterized in that, The hydraulic press in S1 has a pressing pressure of 20~25MPa and a holding time of 20~25s.

4. The method for preparing a high-temperature titanium alloy material with high thermal strength and toughness according to claim 1, characterized in that, In S2, vacuum self-consuming arc melting is performed three times.

5. The method for preparing a high-temperature titanium alloy material with high thermal strength and high toughness according to claim 4, characterized in that, In the three vacuum arc melting processes, the vacuum degree of the first vacuum arc melting process was ≤1.0×10-1 Pa, the melting current was 5~7KA, the melting voltage was 25~35V, and the arc stabilizing current was DC 5A; the vacuum degree of the second vacuum arc melting process was ≤1.0×10-1 Pa, the melting current was 6~8KA, the melting voltage was 23~30V, and the arc stabilizing current was AC 6A / 30s; the vacuum degree of the third vacuum arc melting process was ≤1.0×10-1 Pa, the melting current was 7~9KA, the melting voltage was 25~35V, and the arc stabilizing current was AC 7A / 30s.

6. The method for preparing a high-temperature titanium alloy material with high thermal strength and high toughness according to claim 1, characterized in that, The solution heat treatment temperature is T. β -20~40℃, heat treatment time is 2~4h, and the aging heat treatment temperature is 500~600℃ for 4~8h.

Citation Information

Patent Citations

  • Casting titanium alloy material at 600 DEG C and preparation method thereof

    CN110951993A

  • High-strength titanium alloy used at temperating being 500-600 DEG C and processing method thereof