Polyethylene copolymer for a film layer
By using metallocene-catalyzed multimodal polyethylene copolymers and controlling melt flow rate and density differences through multi-stage polymerization, the problems of uneven processing and insufficient performance of multimodal polyethylene copolymers in membrane applications have been solved, resulting in membrane materials with low sealing initiation temperature and high mechanical properties.
Patent Information
- Application Number
- CN202280044771.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-06-24
- Filing Date
- 2022-06-23
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-06-23
AI Technical Summary
Existing multimodal polyethylene copolymers have problems such as uneven melt processing, high sealing initiation temperature, and insufficient mechanical properties in membrane applications, making it difficult to meet the performance requirements of membrane products.
A multi-peak polyethylene copolymer catalyzed by metallocene catalyst is composed of ethylene-1-butene and ethylene-1-hexene polymer components. By carrying out multi-stage polymerization in different reactors, the melt flow rate and density differences are controlled to form a multi-peak structure, thereby optimizing sealing performance and mechanical properties.
A membrane material with low sealing initiation temperature and high dart strength was achieved, which improved the sealing and mechanical properties of the membrane while maintaining good optical properties.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_5
Abstract
Description
Technical Field
[0001] This invention relates to metallocene-catalyzed multimodal polyethylene copolymers (P), the use of multimodal polyethylene copolymers (P) in membrane applications, and membranes comprising the polymer compositions of this invention. Background Technology
[0002] Single-peak polyethylene (PE) polymers, such as SSC products, are typically used in membrane applications. Single-peak PE polymers possess, for example, good optical properties (such as low haze); however, from a production perspective, the melt processing of such polymers is unsatisfactory and can lead to quality issues in the final product. Multi-peak PE polymers with two or more different polymer components are easier to process, but melt homogenization of multi-peak PEs can be problematic, resulting in non-uniform final products, as evidenced by the high gel content of the final product.
[0003] Borealis' WO 2021009189, WO 2021009190 and WO 2021009191 disclose methods for preparing multi-peak PE polymers in two loop reactors and one gas-phase reactor.
[0004] The total density of the polymer produced in the examples is 938 or 939 kg / m³. 3 The MFR2 (190°C, 2.16 kg, ISO 1133) of the polymer component produced in the first loop was 22 g / 10 min. No mention was made of membrane properties such as the seal initiation temperature (SIT).
[0005] WO 2021009192 also discloses such a method. The polymer produced in the examples has an even higher density, at 951 kg / m³. 3 The MFR2 (190°C, 2.16 kg, ISO 1133) of the polymer component produced in the first loop was 32 g / 10 min. No mention was made of membrane properties such as the seal initiation temperature (SIT).
[0006] WO2021013552, Reference Example RE3 discloses a polymer comprising ethylene-1-butene and ethylene-1-hexene polymer components, produced using bis(1-methyl-3-n-butylcyclopentadienyl)zirconium dichloride (IV) as a metallocene complex in a loop reactor and a gas-phase reactor. Membranes produced from this polymer have a seal initiation temperature (SIT) of 91°C and a dart impact strength of only 345 g.
[0007] WO2021191018 discloses a method for preparing multimodal PE polymers using bis(1-methyl-3-n-butylcyclopentadienyl)zirconium dichloride (IV) as a metallocene complex in two loop reactors and one gas-phase reactor. The polymer produced in the gas-phase reactor according to IE1 has an MFR2 of 1.65 g / 10 min. Membranes made from this polymer exhibit a relatively high haze of 42.2%.
[0008] WO2016083208 again discloses a polymer comprising ethylene-1-butene and ethylene-1-hexene polymer components, which is produced using bis(1-methyl-3-n-butylcyclopentadienyl)zirconium dichloride (IV) as a metallocene complex in a loop reactor and a gas-phase reactor. No mention is made of membrane properties such as seal initiation temperature (SIT) or dart impact strength (DDI).
[0009] US2014194277 discloses blends of two different separately produced (each in only one reactor) polyethylene copolymers (A) and (B). No mention is made of membrane properties such as seal initiation temperature (SIT) or drop dart impact strength (DDI).
[0010] There is a ongoing need to find multi-peaked PE polymers with different performance balances to provide customized solutions that meet the growing demands of end-application manufacturers, such as reducing production costs while maintaining or even improving the performance of the final product. Customized polymer solutions are also needed to meet the evolving equipment technology requirements of end-application sectors.
[0011] Therefore, the prior art needs to provide a material that offers a low sealing initiation temperature, good optical and mechanical properties, and particularly dart resistance (impact strength). In other words, there is a need for a material that provides preferred sealing properties, good optical and mechanical properties, and particularly a favorable combination of SIT, haze, and dart resistance for films prepared from such material. Summary of the Invention
[0012] Therefore, the present invention relates to a metallocene-catalyzed multimodal polyethylene copolymer (P) comprising (i) 30.0 to 70.0 wt% of an ethylene-1-butene polymer component (A) and (ii) 70.0 to 30.0 wt% of an ethylene-1-hexene polymer component (B).
[0013] The ethylene-1-butene polymer component (A) has
[0014] Between 920 and 950 kg / m 3 Density within a certain range
[0015] MFR2 (190 °C, 2.16 kg, ISO 1133) in the range of 2.0 to 40.0 g / 10 min, based on the ethylene-1-butene polymer component (A), with a 1-butene content in the range of 0.5 to 5.0 wt%, and
[0016] The isolated 1-butene comonomer unit content is >95%.
[0017] The amount of the separated 1-butene comonomer unit is calculated according to formula (I).
[0018]
[0019] X is the number of 1-butene branches per 1000 carbons (kCb); and
[0020] The ethylene-1-butene polymer component (A) is composed of an ethylene-1-butene polymer moiety (A-1) and an ethylene-1-butene polymer moiety (A-2), wherein the ethylene polymer moiety (A-1) has...
[0021] Between 920 and 960 kg / m 3 Density within the range, and
[0022] MFR2 (190℃, 2.16 kg, ISO 1133) in the range of 1.0 to 20.0 g / 10 g / 10 min, and
[0023] The ethylene polymer portion (A-2) has
[0024] Between 930 and 950 kg / m 3 The density ranged from 3.0 to 40.0 g / 10 min, and the MFR2 (190°C, 2.16 kg, ISO 1133) was within the range of 3.0 to 40.0 g / 10 min.
[0025] The ethylene polymer component (B) has
[0026] Between 880 and 915 kg / m 3 Density within a certain range
[0027] MFR2 (190 °C, 2.16 kg, ISO 1133), based on ethylene-1-hexene polymer compound (B), with a 1-hexene content ranging from 15.0 to 25.0 wt%, in the range of 0.01 to 1.5 g / 10 min.
[0028] The amount of 1-hexene comonomer units separated according to equation (I), where X is the number of 1-hexene branches per 1000 carbons (kCb); satisfies the equation
[0029] EXE% > -1.1875 * C6((B), in wt%) + 110.41; and
[0030] Among them, multimodal polyethylene copolymer (P) has
[0031] Between 905 and 915 kg / m 3 Density within a certain range
[0032] MFR2 (190°C, 2.16 kg, ISO 1133) in the range of 0.5 to below 2.0 g / 10 min, and
[0033] MFR in the range of 22 to 50 21 The ratio of MFR2 (190°C, 21.6 kg, ISO 1133) to MFR2 (190°C, 2.16 kg, ISO 1133) (MFR 21 / MFR2).
[0034] Surprisingly, the multimodal polyethylene copolymer (P) of the present invention provides the membrane with improved sealing performance (e.g., a particularly low seal initiation temperature (SIT)) and improved membrane mechanical properties (e.g., high dart strength (DDI)).
[0035] Therefore, the present invention further relates to a membrane comprising at least one layer comprising a metallocene-catalyzed multimodal polyethylene copolymer (P).
[0036] The membrane is characterized in that the sealing initiation temperature measured on a 40 μm monolayer test blown film, as described in the experimental section, is below 82°C, preferably in the range of 60°C to 80°C, more preferably in the range of 65°C to 78°C, such as 68°C to 78°C.
[0037] In one embodiment of the invention, in addition to low SIT, the membrane further has a dart impact (DDI) of at least 1000 g and at most 1700 g, preferably at least 1200 g and at most 1700 g, more preferably at least 1500 g and at most 1700 g, as determined according to ASTM D1709, Method A on a 40 μm monolayer test blown film. Attached Figure Description
[0038] Figure 1 This is a graph showing the relationship between the amount of 1-hexene comonomer units isolated and the 1-hexene content in the ethylene-1-hexene polymer component (B). From... Figure 1It is evident that the embodiments of the present invention satisfy the relationship EHE% > -1.1875 * C6 (wt%) + 110.41, while the comparative examples do not. The higher EHE value indicates better comonomer insertion, which is reflected in the greater number of separated 1-hexene units. Detailed Implementation
[0039] definition
[0040] When the term "comprising / including" is used in this specification and claims, it does not exclude other unspecified elements of primary or secondary functional importance. For the purposes of this invention, the term "consisting of..." is considered a preferred embodiment of the term "comprising / including". If a group is defined below as including at least a certain number of embodiments, this should also be understood as a disclosed group, which preferably consists only of these embodiments.
[0041] Whenever the terms “including” or “having” are used, these terms mean equivalent to “include / comprise” as defined above.
[0042] When referring to a singular noun, use the indefinite or definite article, such as "a", "an", or "the / that", unless otherwise specified, this includes the plural form of the noun.
[0043] In this invention, a metallocene-catalyzed multimodal polyethylene copolymer is defined as a multimodal polyethylene copolymer (P), which is produced in the presence of a metallocene catalyst.
[0044] In the context of multimodal polyethylene copolymers (P), the term "multimodal" herein refers to multimodality in relation to the melt flow rate (MFR) of ethylene polymer components (A) and (B) and ethylene polymer portions (A-1) and (A-2), i.e., ethylene polymer components (A) and (B) and portions (A-1) and (A-2) have different MFR values. As described below, multimodal polyethylene copolymers (P) may further possess multimodality in relation to one or more other properties between ethylene polymer components (A) and (B) and between portions (A-1) and (A-2).
[0045] The multimodal polyethylene copolymer (P) of the present invention as defined above, below or in the claims is also referred to herein simply as "multimodal PE" or "multimodal copolymer (P)".
[0046] For the purposes of this invention, "multimodal polyethylene copolymer (P) comprising polyethylene component (A) and polyethylene component (B)" refers to the production of multimodal polyethylene copolymer (P) in a sequential polymerization process of at least two stages, wherein a first component (A) is produced, and then component (B) is produced in a subsequent polymerization step in the presence of component (A) to produce multimodal polyethylene copolymer (P), and vice versa, i.e., a first component (B) is produced, and then component (A) is produced in a subsequent polymerization step in the presence of component (B) to produce multimodal polyethylene copolymer (P).
[0047] Polyethylene produced in a multi-stage process is also known as an "in-situ" or "reactor" blend. The final product consists of an initial mixture of polymers from two or more reactors, whose different molecular weight distributions together form a single molecular weight distribution curve with one broad maximum or two or more maximums; that is, the final product is a multi-peak polymer mixture.
[0048] The following preferred embodiments, properties, and subgroups of multimodal PE and its ethylene polymer components (A) and (B), and its ethylene polymer portions (A-1) and (A-2), as well as the membranes of the present invention including their preferred ranges, are independently generalizable such that they can be used in any order or combination to further define the preferred embodiments of the multimodal PE and articles of the present invention.
[0049] Multimodal PE as well as ethylene polymer components (A) and (B) and ethylene polymer fractions (A-1) and (A-2)
[0050] The multimodal polyethylene copolymer (P) produced by metallocene is referred to herein as "multimodal" because the ethylene-1-butene polymer component (A), comprising ethylene polymer portions (A-1) and (A-2), and the ethylene-1-hexene polymer component (B) have been produced under different polymerization conditions, resulting in different melt flow rates (MFRs, e.g., MFR2). That is, multimodal PE is multimodal at least with respect to the difference in MFR between the ethylene polymer components (A) and (B).
[0051] The multimodal polyethylene copolymer (P) produced by metallocene consists of (i) 30.0 to 70.0 wt% of ethylene-1-butene polymer component (A) and (ii) 70.0 to 30.0 wt% of ethylene-1-hexene polymer component (B).
[0052] The sum of (A) and (B) is 100.0% wt%.
[0053] The ethylene-1-butene polymer component (A) is composed of ethylene polymer parts (A-1) and (A-2), wherein the MFR2 of the ethylene polymer parts (A-1) and (A-2) may be different from each other.
[0054] The MFR2 (190°C, 2.16 kg, ISO 1133) of the ethylene polymer fraction (A-1) is in the range of 1.0 to 20.0 g / 10 min, preferably 1.5 to 18.0 g / 10 min, more preferably 2.0 to 16.0 g / 10 min, and even more preferably 2.5 to 14.0 g / min, such as 3.0 to 12.0 g / 10 min.
[0055] The MFR2 (190°C, 2.16 kg, ISO 1133) of the ethylene polymer fraction (A-2) is in the range of 3.0 to 40.0 g / 10 min, preferably 3.2 to 30.0 g / 10 min, more preferably 3.5 to 20.0 g / 10 min, and most preferably 3.5 to 10.0 g / 10 min.
[0056] The MFR2 of ethylene polymer components (A) and (B) are different from each other.
[0057] The MFR2 (190°C, 2.16 kg, ISO 1133) of the ethylene polymer component (A) is in the range of 2.0 to 40 g / 10 min, preferably 2.5 to 30 g / 10 min, more preferably 3.0 to 20 g / 10 min, and even more preferably 3.2 to 10 g / 10 min.
[0058] The MFR2 (190°C, 2.16 kg, ISO 1133) of the ethylene polymer component (B) is in the range of 0.01 to 1.5 g / 10 min, preferably 0.05 to 1.5 g / 10 min, more preferably 0.1 to 1.2 g / 10 min, and even more preferably 0.2 to 1.0 g / 10 min.
[0059] The MFR2 (190°C, 2.16 kg, ISO 1133) of the multimodal copolymer (P) is in the range of 0.5 to 2.0 g / 10 min, preferably 0.8 to 1.8 g / 10 min, more preferably 1.0 to 1.5 g / 10 min.
[0060] MFR of multimodal copolymer (P) 21 (190°C, 21.6 kg, ISO 1133) and MFR2 (190°C, 2.16 kg) The ratio of kg (ISO 1133) to MFR21 The value of / MFR2) is in the range of 22 to 50, preferably 25 to 40, and more preferably 28 to 35.
[0061] In embodiments of the invention, the preferred MFR2 (190°C, 2.16) of the ethylene-1-butene polymer component (A) is preferred. MFR2 (190°C, 2.16 kg, ISO 1133) and the final multimodal copolymer (P) The ratio of (kg, ISO 1133) is at least 2.5 to 20.0, preferably 3.0 to 15.0, and more preferably 3.5 to 10.0.
[0062] Of course, in addition to the multimodality of the MFR2 (i.e., the difference between them) of the ethylene polymer components (A) and (B), the multimodal PE of the present invention can also be multimodal, for example, with respect to one or both of two other properties:
[0063] Multimodality in terms of the differences between the following:
[0064] - The content of comonomers present in ethylene polymer components (A) and (B); and / or
[0065] - Densities of ethylene polymer components (A) and (B).
[0066] Preferably, the multimodal polymer (P) is further multimodal in terms of the difference in MFR between the ethylene polymer components (A) and (B).
[0067] The polymer parts (A-1) and (A-2) have the same type of comonomer, so both parts have 1-butene as a comonomer.
[0068] The comonomer content of components (A) and (B) can be measured, or, in a preferred case, one component is first produced, and then another component is produced in a so-called multi-stage process in the presence of the first-produced component. The comonomer content of the first-produced component (e.g., component (A)) can then be measured, and the comonomer content of the other component (e.g., component (B)) can be calculated according to the following formula:
[0069] Comonomer content in component B (mol%) = (Comonomer content in the final product (mol%) - (Weight fraction of component A * Comonomer content in component A (mol%)) / (Weight fraction of component B)
[0070] Based on the multimodal polymer (P), the total amount of 1-butene is preferably in the range of 0.1 to 1.0 wt%, more preferably 0.2 to 0.8 wt%, and more preferably 0.3 to 0.6 wt%.
[0071] Based on the multimodal polymer (P), the total amount of 1-hexene is preferably in the range of 2.0 to 20.0 wt%, more preferably 4.0 to 18.0 wt%, and more preferably 6.0 to 15.0 wt%.
[0072] Based on the ethylene-1-butene polymer component (A), the total amount (wt%) of 1-butene present in the ethylene-1-butene polymer component (A) is 0.5 to 5.0 wt%, preferably 0.8 to 4.0 wt%, more preferably 1.0 to 3.0 wt%, and even more preferably 1.0 to 2.0 wt%.
[0073] Based on the ethylene-1-hexene polymer component (B), the total amount (wt%) of 1-hexene present in the ethylene-1-hexene polymer component (B) is 15.0 to 25.0 wt%, preferably 16.0 to 22.0 wt%, more preferably 17.0 to 20.0 wt%.
[0074] Even more preferably, the multimodal polymer (P) of the present invention is further multimodal in terms of the density difference between the ethylene polymer component (A) and the ethylene polymer component (B). Preferably, the density of the ethylene polymer component (A) is different from, and preferably higher than, the density of the ethylene polymer component (B).
[0075] The density of the ethylene polymer component (A) is between 920 and 950 kg / m³. 3 Preferably 925 to 950 kg / m 3 More preferably 930 to 945 kg / m 3 Within the range, and / or the density of the ethylene polymer component (B) is between 880 and 915 kg / m³. 3 Preferred weight is 885 to 905 kg / m³. 3 More preferably 888 to 900 kg / m 3 Within the range.
[0076] The density of the polymer portion (A-1) is between 920 and 960 kg / m³. 3 Preferably 925 to 955 kg / m 3 More preferably 930 to 950 kg / m 3 For example, 935 to 945 kg / m 3 Within the range.
[0077] The density of the polymer portion (A-2) is between 930 and 950 kg / m³. 3 Preferably 935 to 945 kg / m 3 Within the range.
[0078] Metallocene-catalyzed multimodal copolymers (P) are preferably linear low-density polyethylene (LLDPE), which has a well-known meaning.
[0079] The density of the multimodal copolymer (P) is between 905 and 915 kg / m³. 3 Preferably 908.0 to 915 kg / m 3 More preferably 910.0 to 915.0 kg / m 3 Within the range.
[0080] More preferably, the multimodal copolymer (P) is multimodal at least in terms of the MFR2, comonomer content and density of the ethylene polymer components (A) and (B), i.e., having differences as defined above, below or in the claims, including any preferred range or embodiment of the polymer composition.
[0081] Furthermore, the ethylene-1-butene polymer component (A) is characterized by a separated 1-butene comonomer unit content >95.0%, preferably at least 98.0%, and more preferably 100%. The separated comonomer unit content is calculated according to formula (1).
[0082]
[0083] Where X is the number of 1-butene branches per 1000 carbons (kCb).
[0084] Furthermore, the ethylene-1-hexene polymer component (B) has a separated 1-hexene comonomer unit amount according to formula (I), where X is the number of 1-hexene branches per 1000 carbons (kCb); satisfying the equation
[0085] EXE% >-1.1875 * C6((B), in wt%) + 110.41
[0086] Preferably, the ethylene-1-hexene polymer component (B) satisfies the equation
[0087] EXE% >-1.1875 * C6 ((B), in wt%) + 111.41, more preferably
[0088] EXE% >-1.1875 * C6 ((B), in wt%) + 112.41, or even more preferably EXE% >-1.1875 * C6 ((B), in wt%) + 113.41.
[0089] The amount of isolated 1-hexene comonomer units in component (B) is preferably >92.0%, preferably at least 93.0%, and more preferably at least 94.0%.
[0090] The appropriate upper limit is <100%, preferably 99.0%, and more preferably 98.0%.
[0091] Within the scope of this invention, the first and second ethylene polymer portions (A-1 and A-2) of the ethylene polymer component (A) are present in a weight ratio of 4:1 to 1:4, for example 3:1 to 1:3, or 2:1 to 1:2, or 1:1.
[0092] Based on the multimodal copolymer (P), the ethylene polymer component (A) is present in an amount of 30.0 to 70.0 wt%, preferably 32.0 to 55.0 wt%, and even more preferably 34.0 to 45.0 wt%.
[0093] Therefore, based on the multimodal copolymer (P), the ethylene polymer component (B) is present in an amount of 70.0 to 30.0 wt%, preferably 68.0 to 45.0 wt%, and more preferably 66.0 to 55.0 wt%.
[0094] Metallocene-catalyzed multimodal copolymers (P) can be produced using a three-stage process, preferably comprising a first slurry reactor (loop reactor 1) connected in series with another slurry reactor (loop reactor 2), such that a first ethylene polymer fraction (A-1) produced in loop reactor 1 is fed into loop reactor 2, where a second ethylene polymer fraction (A-2) is produced in the presence of the first fraction (A-1). Loop reactor 2 is then connected in series with a gas-phase reactor (GPR), such that the first ethylene polymer component (A) exiting the second slurry reactor is fed into the GPR to produce a trimodal polyethylene copolymer. In this case, the reaction conditions in the two slurry reactors are selected such that products with different MFRs and / or densities are produced in the two reactors.
[0095] This method is described in particular in WO 2016 / 198273, WO 2021009189, WO 2021009190, WO 2021009191 and WO 2021009192. Full details on how to prepare suitable metallocene-catalyzed multimodal copolymers (P) can be found in these references.
[0096] The appropriate process is the Borstar PE process or the Borstar PE 3G process.
[0097] Therefore, the metallocene-catalyzed multimodal copolymer (P) according to the invention is preferably produced in a loop-loop-gas phase cascade. A prepolymerization step may precede such a polymerization step. The purpose of prepolymerization is to polymerize a small amount of polymer onto the catalyst at low temperatures and / or low monomer concentrations. Prepolymerization can improve the performance of the catalyst in the slurry and / or alter the properties of the final polymer. This prepolymerization step is preferably carried out in the slurry, and the amount of polymer produced in the optional prepolymerization step is accounted for as the amount (wt%) of the ethylene polymer component (A).
[0098] When a prepolymerization step is present, it is preferable that all of the catalyst components be introduced into the prepolymerization step. However, when the solid catalyst components and cocatalysts can be fed separately, it is possible that only a portion of the cocatalyst is introduced into the prepolymerization stage, while the remainder is introduced into the subsequent polymerization stage. Furthermore, in this case, it is necessary to introduce so much cocatalyst into the prepolymerization stage in order to achieve sufficient polymerization reaction therein.
[0099] It should be understood that, within the scope of this invention, the amount of polymer produced during prepolymerization is between 1 and 5 wt% relative to the final metallocene-catalyzed multimodal copolymer (P). This can be considered as part of the first ethylene polymer component (A).
[0100] catalyst
[0101] The metallocene-catalyzed multimodal copolymer (P) used in the method of this invention is prepared using a metallocene catalyst. The metallocene catalyst comprises a metallocene complex and a co-catalyst. The metallocene compound or complex is also referred to herein as an organometallic compound (C).
[0102] Organometallic compounds (C) contain transition metals (M) of elements in groups 3 to 10 of the periodic table (IUPAC 2007), or of the actinides or lanthanides.
[0103] According to the present invention, the term "organometallic compound (C)" includes any metallocene or nonmetallocene compound of transition metals, which has at least one organic (coordinating) ligand and exhibits catalytic activity alone or in combination with a co-catalyst. Transition metal compounds are well known in the art, and the present invention covers compounds from Groups 3 to 10 of the periodic table (IUPAC 2007), such as Groups 3 to 7, or Groups 3 to 6, such as Groups 4 to 6, as well as compounds of lanthanides or actinides.
[0104] In one embodiment, the organometallic compound (C) has the following formula (II):
[0105] (II)
[0106] Each X is independently a halogen atom, C 1-6 -alkyl, C 1-6 -alkoxy, phenyl, or benzyl;
[0107] Each Het is independently a monocyclic heteroaromatic group containing at least one heteroatom selected from O or S;
[0108] L is -R'2Si-, where each R' is independently a C substituted with an alkoxy group having 1 to 10 carbon atoms. 1-20 - Hydrocarbon group or C 1-10 -alkyl;
[0109] M is Ti, Zr, or Hf;
[0110] Each R 1 Same or different, is C 1-6 -alkyl or C 1-6 -alkoxy group;
[0111] Each n is between 1 and 2;
[0112] Each R 2 Same or different, is C 1-6 -alkyl, C 1-6 -alkoxy or -Si(R)3 group;
[0113] Each R is arbitrarily selected by 1 to 3 Cs. 1-6 -alkyl-substituted C 1-10 -alkyl or phenyl; and
[0114] Each p is between 0 and 1.
[0115] Preferably, the compound of formula (II) has the following structure
[0116] (II')
[0117] Each X is independently a halogen atom, C 1-6 -alkyl, C 1-6 -alkoxy, phenyl, or benzyl;
[0118] L is Me2Si-;
[0119] Each R 1 Same or different and is C 1-6 -alkyl, such as methyl or tert-butyl;
[0120] Each n is between 1 and 2;
[0121] R 2 It is a -Si(R)3 alkyl group; each p is 1;
[0122] Each R is C 1-6-alkyl or phenyl.
[0123] The highly preferred formula (II) complex is
[0124]
[0125] Most preferably, the complex dimethylsilanediylbis[2-(5-trimethylsilylfuran-2-yl)-4,5-dimethylcyclopentadien-1-yl]zirconium dichloride is used.
[0126] More preferably, the ethylene polymer components (A) and (B) of the multimodal copolymer (P) are prepared using the same metallocene catalyst, i.e., in the presence of the same metallocene catalyst.
[0127] To form the catalyst, a co-catalyst, also known as an activator, is used. Co-catalysts containing Al or B are well known and can be used here. Aluminoxanes (e.g., MAO) or boron-based co-catalysts (e.g., borates) are preferred.
[0128] In contrast to Ziegler-Natta catalysis, polyethylene copolymers prepared using site-specific catalysis exhibit characteristics that distinguish them from Ziegler-Natta materials. In particular, the comonomer distribution is more uniform. This can be visualized using TREF or Crystaf techniques. Catalyst residues can also indicate the catalyst used. Ziegler-Natta catalysts do not contain, for example, Zr or Group IV (Hf) metals.
[0129] Metallocene-catalyzed multimodal copolymers (P) may contain other polymer components and optional additives and / or fillers. When metallocene-catalyzed multimodal copolymers (P) contain other polymer components, the amount of the other polymer components typically varies between 3.0 and 20.0 wt%, depending on the total amount of the metallocene-catalyzed multimodal copolymer (P) and the other polymer components.
[0130] Optional additives and fillers, and their amounts, are common in membrane applications. Examples of such additives include antioxidants, processing stabilizers, UV stabilizers, pigments, fillers, antistatic additives, antiblocking agents, nucleating agents, acid scavengers, and polymer processing aids (PPAs).
[0131] It should be understood here that any additives and / or fillers may optionally be added to a so-called masterbatch containing the corresponding additives and carrier polymers. In this case, based on the total amount (100 wt%) of the polymer composition, the carrier polymer is not calculated in the polymer component of the metallocene-catalyzed multimodal copolymer (P), but rather in the amount of the corresponding additives.
[0132] The membrane of the present invention
[0133] The membrane of the present invention comprises at least one layer containing a metallocene-catalyzed multimodal copolymer (P). The membrane may be a monolayer membrane containing a metallocene-catalyzed multimodal copolymer (P) or a multilayer membrane wherein at least one layer contains a metallocene-catalyzed multimodal copolymer (P). The terms "monolayer membrane" and "multilayer membrane" have well-known meanings in the art.
[0134] The single-layer or multi-layer membranes of the present invention may consist of the metallocene-catalyzed multimodal copolymer (P) itself, or a blend of the metallocene-catalyzed multimodal copolymer (P) with other polymers. In the case of blends, any other polymer is different from the metallocene-catalyzed multimodal copolymer (P), and is preferably a polyolefin. A portion of the aforementioned additives, such as processing aids, may optionally be added to the metallocene-catalyzed multimodal copolymer (P) during the membrane preparation process.
[0135] Preferably, at least one layer of the present invention comprises at least 50 wt%, more preferably at least 60 wt%, even more preferably at least 70 wt%, and still more preferably at least 80 wt% of the metallocene-catalyzed multimodal copolymer (P) of the present invention. Most preferably, the at least one layer of the membrane of the present invention is composed of a metallocene-catalyzed multimodal copolymer (P).
[0136] Therefore, the membrane of the present invention may comprise a single layer (i.e., a monolayer) or may comprise multiple layers. Multilayer membranes typically and preferably comprise at least three layers.
[0137] The film is preferably produced by any conventional film extrusion process known in the art, including cast film and blown film extrusion. Most preferably, the film is a blown or cast film, especially a blown film. For example, a blown film is produced by extrusion via an annular die and by blowing a tubular film by forming bubbles, which then rupture between rolls after solidification. The film can then be cut, diced, or converted (e.g., folded) as needed. Conventional film production techniques can be used in this regard. If the preferred blown or cast film is a multilayer film, then the layers are typically co-extruded. Those skilled in the art will know the appropriate extrusion conditions.
[0138] The membrane according to the invention can undergo post-processing, such as surface modification, lamination, or orientation processes. Such orientation processes can be uniaxial (MDO) or biaxial orientation, with uniaxial orientation being preferred.
[0139] In another preferred embodiment, the membrane is non-oriented.
[0140] The resulting membrane can have any thickness conventional in the art. The membrane thickness is not critical and depends on the end application. Therefore, the membrane can have a thickness of, for example, 300 μm or less, typically 6 to 200 μm, preferably 10 to 180 μm, such as 20 to 150 μm or 20 to 120 μm. If desired, the polymers of the present invention can achieve thicknesses of less than 100 μm, for example, less than 50 μm. Membranes of the present invention with thicknesses even less than 20 μm can also be produced while maintaining good mechanical properties.
[0141] Furthermore, the present invention relates to the use of the articles of the invention as packaging materials, particularly as packaging materials for food and / or medical products.
[0142] The membrane of the present invention is characterized in that the sealing initiation temperature measured on a blown film with a thickness of 40 μm as described in the experimental section is below 82°C, preferably in the range of 60°C to 80°C, more preferably in the range of 65°C to 78°C, such as 68°C to 78°C.
[0143] In the embodiments, the membrane comprising the metallocene-catalyzed multimodal copolymer (P) is further characterized by a dart impact strength (DDI) of at least 1000 g to greater than 1700 g, preferably 1200 g to greater than 1700 g, and more preferably 1500 g to greater than 1700 g, as determined by ASTM D1709 Method A on a 40 μm monolayer test blown film.
[0144] The upper limit of "greater than 1700 g" is because the detection limit of the corresponding method is 1700 g.
[0145] Therefore, in a preferred embodiment, the membrane comprising a metallocene-catalyzed multimodal polyethylene copolymer (P) is characterized by having at least […].
[0146] a) A sealing initiation temperature below 82°C, preferably in the range of 60°C to 80°C, and more preferably in the range of 65°C to 78°C, as measured on a blown film with a thickness of 40 μm, as described in the experimental section, such as 68°C to 78°C.
[0147] and
[0148] b) According to ASTM D1709, Method A, at least 1000 g on a 40 μm monolayer test blown film is measured.
[0149] The dart impact intensity (DDI) is at most 1700 g, preferably 1200 g, and more preferably 1500 g.
[0150] Furthermore, the film according to the invention has good stiffness (tensile modulus measured on a 40 μm monolayer blown film according to ISO 527-3), i.e., >150 MPa (in both directions) and good optical properties, i.e., haze (measured on a 40 μm monolayer blown film according to ASTM D1003-00) less than 25%.
[0151] Therefore, the film containing the metallocene-catalyzed multimodal copolymer (P) can further or additionally have a haze of less than 25%, preferably 5% to 24%, more preferably 10% to 22% (measured on a 40 μm monolayer test blown film according to ASTM D 1003-00), and a tensile modulus in the longitudinal (MD) and transverse (TD) directions in the range of >150 MPa to 300 MPa, preferably >150 MPa to 250 MPa (measured on a 40 μm monolayer test blown film according to ISO 527-3).
[0152] The present invention will be further described with reference to the following non-limiting embodiments.
[0153] Determination methods
[0154] Unless otherwise stated in the instructions or experimental section, the following methods are used to determine the performance of polymers (including their parts and components) and / or any sample formulations thereof as described in the text or experimental section.
[0155] melt flow rate
[0156] Melt flow rate (MFR) is determined according to ISO 1133 and expressed in g / 10 min. MFR is an indicator of polymer flowability and therefore also an indicator of polymer processing performance. A higher melt flow rate generally indicates a lower polymer viscosity. The MFR of polyethylene is determined at 190°C. MFR can be determined under different loads, such as 2.16 kg (MFR2), 5 kg (MFR5), or 21.6 kg (MFR6). 21 ).
[0157] Calculation of MFR2 for component B and part (A-2)
[0158]
[0159]
[0160] For component B:
[0161] B = MFR2 of component (A)
[0162] C = MFR2 of component (B)
[0163] A = Final MFR2 (mixture) of multimodal polyethylene copolymer (P)
[0164] X = weight fraction of component (A)
[0165] For part (A-2):
[0166] B = MFR2 of Part 1 (A-1)
[0167] C = MFR2 of Part 2 (A-2)
[0168] A = final MFR2 (mixture) of cyclic polymer (= component (A))
[0169] X = weight fraction of part 1 (A-1)
[0170] density
[0171] The density of the polymer was determined according to ASTM D792, Method B (equilibrium density at 23°C) on compression-molded specimens prepared according to EN ISO 1872-2, in kg / m³.
[0172] Comonomer content:
[0173] Quantitative analysis of microstructure using NMR spectroscopy
[0174] Quantitative nuclear magnetic resonance (NMR) spectroscopy is used to quantify the comonomer content of polymers.
[0175] Using a Bruker Avance III 500 NMR spectrometer, the NMR spectrometer was used to measure the NMR spectrometer at 500.13 and 125.76 MHz. 1 H and 13 C performs the operation, recording a quantitative value in the molten state. 13 C{ 1 H NMR spectroscopy. All spectra were performed using H NMR spectroscopy. 13 Recordings were performed using a C-optimized 7 mm magic angle rotation (MAS) probe at 150 °C, with all pneumatic setups using nitrogen. Approximately 200 mg of material was loaded into a 7 mm outer diameter (d) zirconia MAS rotor and rotated at 4 kHz. This setup was chosen primarily for the high sensitivity required for rapid identification and accurate quantification. Standard single-pulse excitation was employed, utilizing a 3 s short-cycle delay NOE with an RS-HEPT decoupling scheme. A total of 1024 (1 k) transients were obtained for each spectrum.
[0176] Quantitative13 C{ 1 The ¹H NMR spectra were processed, integrated, and the relevant quantitative characteristics were determined by integration. All chemical shifts were performed with the bulk methylene signal (δ+) at 30.00 ppm as an internal reference.
[0177] The amount of ethylene was quantified by integrating the number of methylene (δ+) sites per monomer reporter site at 30.00 ppm:
[0178] E = I δ+ / 2
[0179] The presence of isolated comonomer units is corrected based on the number of existing isolated comonomer units: Etotal = E + (3*B + 2*H) / 2
[0180] B and H are defined for their respective comonomers. Corrections are made in a similar manner when continuous and discontinuous comonomers are incorporated.
[0181] Observing the characteristic signal corresponding to the incorporation of 1-butene, the comonomer fraction was calculated as the fraction of 1-butene in the polymer relative to all monomers in the polymer:
[0182] fB total = B total / (E total + B total + H total)
[0183] The amount of isolated 1-butene incorporated into the EEBEE sequence was quantified by integrating the B2 site at 39.8 ppm as a percentage of the number of reporter sites per comonomer:
[0184] B = I *B2
[0185] If present, the amount of sequentially incorporated 1-butene in the EEBBEE sequence is quantified by the integral of the ααB2B2 site at 39.4 ppm relative to the number of reporter sites per comonomer:
[0186] BB = 2 * IααB2B2
[0187] The amount of discontinuous 1-butene incorporated into the EEBBEE sequence was quantified by integrating the ββB2B2 site at 24.6 ppm as a percentage of the number of reporter sites per comonomer:
[0188] BEB = 2 * IββB2B2
[0189] Since the *B2 and *βB2B2 sites of the isolated (EEBEE) and discontinuously incorporated (EEBEBEE) 1-butene overlap, the total amount of isolated 1-butene incorporated is corrected for the amount of discontinuous 1-butene present:
[0190] B = I *B2 - 2 * I ββB2B2
[0191] No BBB sequence was observed. The total 1-butene content was calculated based on the sum of isolated, continuous, and discontinuously incorporated 1-butene:
[0192] Total B = B + BB + BEB
[0193] Then calculate the total mole fraction of 1-butene in the polymer:
[0194] fB = B total / (E total + B total + H total)
[0195] Characteristic signals corresponding to 1-hexene incorporation were observed, and the comonomer fraction was calculated as the fraction of 1-hexene in the polymer relative to all monomers in the polymer:
[0196] fH total = H total / (E total + B total + H total)
[0197] The amount of isolated 1-hexene incorporated into the EEHEE sequence was quantified by integrating the B4 site at 38.3 ppm as a percentage of the number of reporter sites per comonomer:
[0198] H = I *B4
[0199] If present, the amount of sequentially incorporated 1-hexene in the EEHHEE sequence is quantified by the integral of the ααB4B4 site at 40.5 ppm relative to the number of reporter sites per comonomer:
[0200] HH = 2 * IααB4B4
[0201] If present, the amount of discontinuously incorporated 1-hexene in the EEHEHEE sequence is quantified by the integral of the ββB4B4 site at 24.7 ppm relative to the number of reporter sites per comonomer:
[0202] HEH = 2 * IββB4B4
[0203] No HHH sequence was observed. The total 1-hexene content was calculated based on the sum of isolated, continuous, and discontinuously incorporated 1-hexene:
[0204] H total = H + HH + HEH
[0205] Then calculate the total mole fraction of 1-hexene in the polymer:
[0206] fH = H total / (E total + B total + H total)
[0207] The molar percentage of comonomer incorporated is calculated from the mole fraction:
[0208] B [mol%] = 100 * fB
[0209] H [mol%] = 100 * fH
[0210] The weight percentage of comonomer incorporated is calculated as a mole fraction:
[0211] B [wt%]= 100 *(fB * 56.11) / ((fB * 56.11)+(fH * 84.16)+((1-(fB+fH))*28.05))
[0212] H [wt%] = 100 * ( fH * 84.16 ) / ( (fB * 56.11) + (fH * 84.16) + ((1-(fB + fH)) * 28.05) )
[0213] References:
[0214] Klimke, K., Parkinson, M., Piel, C., Kaminsky, W., Spiess, HW,Wilhelm, M., Macromol. Chem. Phys. 2006;207:382.
[0215] Parkinson, M., Klimke, K., Spiess, HW, Wilhelm, M., Macromol. Chem. Phys. 2007;208:2128.
[0216] Pollard, M., Klimke, K., Graf, R., Spiess, HW, Wilhelm, M., Sperber, O., Piel, C., Kaminsky, W., Macromolecules 2004;37:813.
[0217] Filip, X., Tripon, C., Filip, C., J. Mag. Resn. 2005, 176, 239
[0218] Griffin, JM, Tripon, C., Samoson, A., Filip, C., and Brown, SP,Mag. Res. in Chem. 2007 45, S1, S198
[0219] Castignolles, P., Graf, R., Parkinson, M., Wilhelm, M., Gaborieau, M., Polymer 50 (2009) 2373
[0220] Busico, V., Cipullo, R., Prog. Polym. Sci. 26 (2001) 443
[0221] Busico, V., Cipullo, R., Monaco, G., Vacatello, M., Segre, AL, Macromoleucles 30 (1997) 6251
[0222] Zhou, Z., Kuemmerle, R., Qiu, X., Redwine, D., Cong, R., Taha, A., Baugh, D. Winniford, B., J. Mag. Reson. 187 (2007) 225
[0223] Busico, V., Carbonniere, P., Cipullo, R., Pellecchia, R., Severn, J.,Talarico, G., Macromol. Rapid Commun. 2007, 28, 1128
[0224] Resconi, L., Cavallo, L., Fait, A., Piemontesi, F., Chem. Rev. 2000,100, 1253
[0225] Sealing start temperature (SIT); Sealing end temperature (SET); Sealing range:
[0226] This method determines the sealing temperature range (sealing range) for polyethylene films, particularly blown or cast films. The sealing temperature range is the temperature range within which the film can be sealed according to the conditions given below.
[0227] The lower limit (heat seal initiation temperature (SIT)) is the sealing temperature at which a seal strength ≥ 5 N is achieved. The upper limit (seal end temperature (SET)) is reached when the membrane adheres to the sealing device.
[0228] Measurements were performed according to a slightly modified version of ASTM F1921–12, with modifications made to the test parameters: sealing pressure, cooling time, and test speed. The force / temperature profile was continued until thermal failure of the membrane.
[0229] The sealing range was determined on a J&B General Seal Machine Model 4000 using a blown film with a thickness of 40 μm, and includes the following further parameters:
[0230] Adjustment time: >96 h
[0231] Sample width: 25 mm
[0232] Sealing pressure: 0.4 N / mm² (PE)
[0233] Sealing time: 1 sec
[0234] Delay time: 30 sec
[0235] Sealing clamp size: 50 x 5 mm
[0236] Sealing clamp shape: flat
[0237] Sealing clamp coating: Niptef
[0238] Sealing temperature: Ambient temperature -240°C
[0239] Sealing temperature interval: 5°C
[0240] Starting temperature: 50°C
[0241] Clamping separation rate: 42 mm / sec
[0242] Dart Drop Intensity (DDI)
[0243] Dart dropping measurements were performed on the membranes produced as shown below using ASTM D1709 Method A (Alternative Test Technique). Darts with a hemispherical head and a diameter of 38 mm were dropped from a height of 0.66 m onto the multilayer membrane clamped in a hole. Twenty sets of samples were tested consecutively. One weight was used for each set, and the weight increased (or decreased) in uniform increments between sets. The weight that caused 50% of the samples to break was calculated and reported.
[0244] Membrane sample preparation
[0245] Test films with a thickness of 40 μm, composed of the multimodal copolymer (P) of this invention and their respective comparative polymers, were prepared using a Collin 30 laboratory-scale single-layer blown film production line. The film samples were produced at 194 °C, a blown ratio of 1:2.5, and a frosting line distance of 120 mm.
[0246] Experimental Section
[0247] Example: Preparation of catalysts for IE1 and IE2 (CAT1)
[0248] SiO2 loading:
[0249] Add 10 kg of silica (PQ Corporation ES757, calcined at 600°C) from the feed hopper and inertize it in the reactor until the O2 level is below 2 ppm.
[0250] Preparation of MAO / tol / MC:
[0251] At 25°C (oil circulation temperature) and with stirring at 95 rpm, 30 wt% MAO from toluene (14.1 kg) was added from a balance to another reactor, followed by the addition of toluene (4.0 kg). After the addition of toluene, the stirring speed was increased from 95 rpm to 200 rpm for 30 minutes. 477 g of metallocene racemic dimethylsilanediylbis{2-(5-(trimethylsilyl)furan-2-yl)-4,5-dimethylcyclopentadien-1-yl}zirconium dichloride was added from a metal cylinder, followed by rinsing with 4 kg of toluene (total toluene 8.0 kg). The reactor stirring speed was changed to 95 rpm for MC feed, then returned to 200 rpm and maintained for 3 hours. After the reaction time, the MAO / tol / MC solution was transferred to a feed vessel.
[0252] Preparation of catalysts:
[0253] The reactor temperature was set to 10°C (oil circulation temperature) and the mixture was stirred at 40 rpm with MAO / tol / MC added. The MAO / tol / MC solution (target 22.5 kg, actual 22.2 kg) was added over 205 min, followed by stirring for 60 min (oil circulation temperature set to 25°C). After stirring, the "dry mixture" was stabilized at 25°C (oil circulation temperature) for 12 h with a stirring speed of 0 rpm. The reactor was rotated 20° (back and forth) and stirred several times per hour at 5 rpm.
[0254] After stabilization, the catalyst was dried at 60°C (oil circulation temperature) for 2 hours under a nitrogen flow of 2 kg / h, followed by vacuum drying for 13 hours (with the same nitrogen flow and stirring at 5 rpm). Samples of the dried catalyst were taken, and the HC content was measured using thermogravimetric analysis with a Sartorius moisture analyzer (model MA45) in a glove box. The target HC level was <2% (actual 1.3%).
[0255] Comparative catalyst (CAT2)
[0256] As catalyst CAT2, a supported catalyst containing aluminoxane was used, which contains metallocene di(1-methyl-3-n-butylcyclopentadienyl)zirconium chloride (IV) and features enhanced ActivCat® activator technology from Grace.
[0257] Polymerization: Embodiment of the present invention: The multimodal polyethylene copolymer (P) of the present invention having 1-butene and 1-hexene comonomers.
[0258] The Borstar pilot plant consists of a three-reactor unit (loop 1 – loop 2 – GPR1) and a prepolymer loop reactor.
[0259] The multimodal copolymers (P) of the present invention in Examples 1 (IE1) to 2 (IE1, IE2) and the multimodal polymers (P) of the comparative examples (CE1 to CE4) were produced by using the polymerization conditions given in Table 1.
[0260] Table 1: Aggregation Conditions
[0261] CE1 CE2 CE3 CE4 IE1 IE2 <![CDATA[ Prepolymerization reactor ]]> catalyst CAT2 CAT2 CAT2 CAT2 CAT1 CAT1 Catalyst feed (g / h) 29.0 29.5 29.4 17.0 35 35 Temperature (°C) 50.0 50.0 50.0 50.0 50 50 Pressure (kPa) 5718.9 5702.4 5687.0 5692.4 5639 5617 C2 (kg / h) 4.0 4.0 4.0 4.0 4.0 4.0 H2(g / h) 0.0 0.0 0.0 0.0 0.04 0.03 C4 (g / h) 168.4 169.8 166.1 176.3 81.9 80.6 Split (wt%) 2.7 2.8 2.8 2.7 3.4 3.5 <![CDATA[ Ring pipe section 1 (A-1) ]]> Temperature (°C) 85 85 85 85 85 85 Pressure (kPa) 5557.6 5556.3 5553.6 5525.5 5544 5537 C2 concentration (mol%) 3.1 3.3 3.1 3.5 3.5 3.7 H2 / C2 ratio (mol / kmol) 0.2 0.2 0.2 0.1 0.41 0.50 C4 / C2 ratio (mol / kmol) 85.4 75.9 77.6 33.6 41 40 Splits (wt%) 17.2 17.9 17.5 15.6 17.6 17.8 Density (kg / m3) of material in ring pipe 1 (partial (A-1)) 938 940.5 940 940 941 943 MFR2 (kg / 10 min) of material for loop 1 (part (A-1)) 3.2 7.1 6.2 0.8 5.0 10.0 <![CDATA[ Ring pipe 2 ]]> Temperature (°C) 85.0 85.0 85.0 85.0 85 85 Pressure (kPa) 5365.5 5366.3 5360.8 5333.4 5325 5337 C2 concentration (mol%) 3.1 3.2 3.1 2.7 3.5 4.1 H2 / C2 ratio (mol / kmol) 0.1 0.1 0.1 0.3 0.6 0.5 C4 / C2 ratio (mol / kmol) 88.4 83.7 85.5 201.5 29 28 Splits (wt%) 19.2 20.3 19.8 18.9 20.4 20 Density (kg / m3) of component (A) after loop 2 938.5 941.4 940.9 942.0 940.7 942.3 MFR2 (kg / 10 min) after loop 2 (component (A)) 3.5 8.4 7.3 6.3 5.8 7.5 MFR2 (kg / 10 min) of material for loop 2 (part (A-2)) 3.7 10 8.6 45 6.8 5.5 Density (kg / m3) of material in ring pipe 2 (partial (A-2)) 939 942 942 944 941 941 C4 (wt%) of the material after loop 2 (component (A)) 1.03 0.98 1.00 1.08 1.21 1.21 <![CDATA[ GPR ]]> Temperature (°C) 75.0 75.0 75.0 75.0 75.0 75 Pressure (kPa) 2000.1 2000.2 1999.8 2000.0 2000.0 2000 H2 / C2 ratio (mol / kmol) 0.2 0.2 0.3 0.2 1.18 1.05 C6 / C2 ratio (mol / kmol) 36.2 39.8 37.9 30.3 14.5 14.04 Splits (wt%) 61.0 59.0 60.0 62.8 58.6 58.7 MFR2 (g / 10 min) of GPR material (component (B)) 0.6 0.5 0.9 0.3 0.5 0.3 Density (g / m3) of GPR material (component (B)) 899 896 898 902 891 891 C6 (wt%) of GPR material (component (B)) 15.41 16.27 15.67 13.22 18.60 18.23
[0262] The polymer was mixed with 2400 ppm of Irganox B561 and 270 ppm of Dynamar FX 5922, compounded and extruded into granules using a JSW extruder under a nitrogen atmosphere, resulting in an SEI of 230 kWh / kg and a melt temperature of 192°C.
[0263] Table 2: Material properties and membrane parameters of the multimodal copolymer (P) of the present invention and the comparative copolymer
[0264] Material CE1 CE2 CE3 CE4 IE1 IE2 <![CDATA[MFR2 (g / 10 min) (final)]]> 1.2 1.5 2.1 1.0 1.3 1.0 <![CDATA[MFR 21 (g / 10 min)]]> 22.9 32.5 44.8 19.8 38.7 30.1 <![CDATA[MFR 21 / MFR2]]> 19.1 21.7 21.3 19.8 29.8 30.1 <![CDATA[Density (kg / m 3 )]]> 915 914.5 915 917 913 913 C4 (wt%) 0.4 0.4 0.4 0.4 0.5 0.5 C6 (wt%) 9.6 9.6 9.4 8.3 10.7 10.9 <![CDATA[MFR2(A) / MFR2(final)]]> 3.1 6.4 4.0 6.36 4.5 7.5 EBE (kCb) 1.1 1.1 1.1 0.9 1.3 1.3 EBB (kCb) 0 0 0 0 0 0 BBB (kCb) 0 0 0 0 0 0 EBE (%) 100 100 100 100 100 100 EHE (kCb) 13.2 12.6 11.9 11.7 16 15.2 EHH (kCb) 1.2 1.3 1 0.6 0.9 0.8 HHH (kCb) 0 0 0 0 0 0 EHE (%) 91.7 90.6 92.2 95.1 94.7 95.0 Membrane properties SIT [°C] 70 71 73 88 71 70 DDI [g] 1090 1110 712 1100 >1700 >1700 Tensile modulus (MPa) (MD / TD) 167 / 190 191 / 192 193 / 211 196 / 220 155 / 158 156 / 170 Haze 8.8 13.6 19.3 13.5 16.6 21.5
[0265] Figure 1 The embodiments of the present invention shown in the figure satisfy the following relationship
[0266] EHE% > -1.1875 * C6 (wt%) + 110.41, while the comparative example has no such result.
[0267] A higher EHE value indicates better comonomer insertion, which is reflected in more isolated 1-hexene units.
[0268] As can be clearly seen from the table above, the film composed of the multi-peak copolymer (P) of the present invention exhibits a significantly higher DDI compared to the comparative example.
[0269] In addition, such membranes have improved overall performance, including comparable seal initiation temperature (SIT), good rigidity, and good haze, but with significantly improved DDI.
Claims
1. A metallocene-catalyzed multimodal polyethylene copolymer (P), which comprises the following: (i) 30.0 to 70.0 wt% of ethylene-1-butene polymer component (A), and (ii) 70.0 to 30.0 wt% of ethylene-1-hexene polymer component (B), The ethylene-1-butene polymer component (A) has Between 920 and 950 kg / m 3 Density within a certain range MFR2 in the range of 2.0 to 40.0 g / 10 min, determined according to ISO 1133 at 190 °C and 2.16 kg. Based on the ethylene-1-butene polymer component (A), the 1-butene content ranges from 0.5 to 5.0 wt%, and >95% of the isolated 1-butene monomer units The amount of the separated 1-butene monomer unit is calculated according to formula (I). (I) Where EXE represents the number of 1-butene units surrounded by two ethylene units, EXX represents the number of 1-butene units surrounded by one ethylene unit and one 1-butene unit, and XXX represents the number of 1-butene units surrounded by two 1-butene units; and The ethylene-1-butene polymer component (A) is composed of an ethylene-1-butene polymer moiety (A-1) and an ethylene-1-butene polymer moiety (A-2). The ethylene-1-butene polymer portion (A-1) has Between 920 and 960 kg / m 3 Density within the range; as well as MFR2 in the range of 1.0 to 20.0 g / 10 min, said MFR2 determined according to ISO 1133 at 190 °C and 2.16 kg, and The ethylene-1-butene polymer portion (A-2) has Between 930 and 950 kg / m 3 The density within the range of 3.0 to 40.0 g / 10 min, and the MFR2, determined according to ISO 1133 at 190 °C and 2.16 kg. The ethylene-1-hexene polymer component (B) has Between 880 and 915 kg / m 3 Density within a certain range MFR2 in the range of 0.01 to 1.5 g / 10 min, determined according to ISO 1133 at 190 °C and 2.16 kg. Based on the ethylene-1-hexene polymer component (B), the 1-hexene content ranges from 15.0 to 25.0 wt%. The amount of 1-hexene monomer units separated according to formula (Ia), (him) Where EYE represents the number of 1-hexene units surrounded by two ethylene units, EYY represents the number of 1-hexene units surrounded by one ethylene unit and one 1-hexene unit, and YYY represents the number of 1-hexene units surrounded by two 1-hexene units; satisfying the equation EYE% > -1.1875 * C6(B) + 110.41, where C6(B) is the 1-hexene content in the ethylene-1-hexene polymer component (B) in wt%; and The multimodal polyethylene copolymer (P) has Between 905 and 915 kg / m 3 Density within a certain range MFR2 in the range of 0.5 to below 2.0 g / 10 min, determined according to ISO 1133 at 190 °C and 2.16 kg, and MFR in the range of 22 to 50 21 The ratio of MFR to MFR2 21 / MFR2, wherein the MFR2 is determined according to ISO 1133 at 190°C and 2.16 kg, wherein the MFR 21 Determined according to ISO 1133 at 190°C and 21.6 kg.
2. The metallocene-catalyzed multimodal polyethylene copolymer (P) according to claim 1, wherein the multimodal polyethylene copolymer (P) is a reactor blend produced in a three-stage sequential polymerization process.
3. The metallocene-catalyzed multimodal polyethylene copolymer (P) according to claim 1 or 2, wherein... - The MFR2 of the ethylene-1-butene polymer component (A) is 2.5 to 30 g / 10 min, and the MFR2 is determined according to ISO 1133 at 190 °C and 2.16 kg. The ethylene-1-butene polymer portion (A-1) has Between 925 and 955 kg / m 3 Density within the range; and MFR2 in the range of 1.5 to 18.0 g / 10 min, determined according to ISO 1133 at 190 °C and 2.16 kg. The ethylene-1-butene polymer portion (A-2) has Between 935 and 945 kg / m 3 The density within the range of 3.2 to 30.0 g / 10 min, and the MFR2 determined according to ISO 1133 at 190 °C and 2.16 kg; and - The MFR2 of the ethylene-1-hexene polymer component (B) is 0.05 to 1.5 g / 10 min, and the MFR2 is determined according to ISO 1133 at 190 °C and 2.16 kg.
4. The metallocene-catalyzed multimodal polyethylene copolymer (P) according to claim 1 or 2, wherein the MFR 21 The ratio of MFR to MFR2 21 / MFR2 is in the range of 25 to 40, and the MFR2 is determined according to ISO 1133 at 190°C and 2.16 kg. 21 Determined according to ISO 1133 at 190°C and 21.6 kg.
5. The metallocene-catalyzed multimodal polyethylene copolymer (P) according to claim 1 or 2, wherein the total amount of 1-butene based on the multimodal polyethylene copolymer (P) ranges from 0.1 to 1.0 wt%, and Based on the multimodal polyethylene copolymer (P), the total amount of 1-hexene ranges from 2.0 to 20.0 wt%.
6. The metallocene-catalyzed multimodal polyethylene copolymer (P) according to claim 1 or 2, wherein, based on the ethylene-1-butene polymer component (A), the total amount (wt%) of 1-butene present in the ethylene-1-butene polymer component (A) is from 0.8 to 4.0 wt%, and Based on the ethylene-1-hexene polymer component (B), the total amount of 1-hexene present in the ethylene-1-hexene polymer component (B) is 16.0 to 22.0 wt%.
7. The metallocene-catalyzed multimodal polyethylene copolymer (P) according to claim 1 or 2, wherein the ethylene-1-butene polymer component (A) is present in an amount of 32.0 to 55.0 wt% based on the multimodal polyethylene copolymer (P), and The ethylene-1-hexene polymer component (B) is present in an amount of 68.0 to 45.0 wt% based on the multimodal polyethylene copolymer (P).
8. The metallocene-catalyzed multimodal polyethylene copolymer (P) according to claim 1 or 2, wherein the multimodal polyethylene copolymer (P) is produced in the presence of a metallocene complex of formula (II): (II) Each X is independently a halogen atom, C 1-6 -alkyl, C 1-6 -alkoxy, phenyl, or benzyl; Each Het is independently a monocyclic heteroaromatic group containing at least one heteroatom selected from O or S; L is -R'2Si-, where each R' is independently a C substituted with an alkoxy group having 1 to 10 carbon atoms. 1-20 - Hydrocarbon group or C 1-10 -alkyl; M is Ti, Zr, or Hf; Each R 1 Same or different, is C 1-6 -alkyl or C 1-6 -alkoxy group; Each n is between 1 and 2; Each R 2 Same or different, is C 1-6 -alkyl, C 1-6 -alkoxy or -Si(R)3 group; Each R is arbitrarily selected by 1 to 3 Cs. 1-6 -alkyl-substituted C 1-10 -alkyl or phenyl; and Each p is between 0 and 1.
9. A membrane comprising a metallocene-catalyzed multimodal polyethylene copolymer (P) according to any one of claims 1 to 8.
10. The membrane of claim 9, wherein the membrane comprises at least one layer comprising a metallocene-catalyzed multimodal polyethylene copolymer (P), wherein the at least one layer comprises at least 50 wt% of the metallocene-catalyzed multimodal polyethylene copolymer (P) according to any one of claims 1 to 8.
11. The membrane according to claim 9 or 10, wherein the membrane is characterized in that the sealing initiation temperature measured on a blown film with a thickness of 40 μm is below 82°C.
12. The membrane according to claim 9 or 10, wherein the membrane is characterized in that the dart impact strength, determined by method A according to ASTM D1709, on a 40 μm monolayer test blown film is at least 1000 g and at most 1700 g.
13. The film according to any one of claims 9 to 12, used as packaging material.
Citation Information
Patent Citations
Ethylene-based polymer, polyethylene-based resin composition and use thereof, catalyst component for olefin polymerization, olefin polymerization catalyst containing the component, and method for producing ethylene-based polymer by using the catalyst
US20140194277A1
Polyethylene composition for a film layer
WO2016083208A1
Multimodal copolymer of ethylene and at least two alpha-olefin comonomers and final articles made thereof
WO2016198273A1
Process for producing a polymer composition
WO2021009189A1
Process for producing a polymer composition
WO2021009190A1