A sulfonate-containing crosslinked polyimide hollow fiber gas separation membrane and a method for preparing the same
By blending polyimide materials and performing low-temperature crosslinking treatment, a hollow fiber gas separation membrane with high mechanical strength and resistance to plasticization was prepared, solving the problems of membrane micropore collapse and heavy hydrocarbon plasticization in existing technologies, and achieving high-throughput and selective gas separation effects.
Patent Information
- Application Number
- CN202311571651.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-23
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-11-23
AI Technical Summary
Existing polyimide hollow fiber gas separation membranes are prone to micropore collapse during high-temperature cross-linking treatment, which reduces flux and selectivity. Furthermore, the plasticizing effect of heavy hydrocarbon components affects separation performance, and membrane material stability issues exist, especially in applications involving natural gas/associated gas, flue gas, and biogas.
A blended polyimide hollow fiber gas separation membrane with a sulfonate crosslinking structure is prepared by blending two polyimide materials, one with hydroxyl groups and the other with acidic functional groups, using a non-solvent phase inversion method. The membrane is then crosslinked by esterification under conditions below the glass transition temperature to form a stable crosslinked structure.
The mechanical strength and anti-plasticization ability of hollow fiber gas separation membranes have been improved, while maintaining high gas permeation flux and selectivity, thus solving the stability problem of membrane materials in practical applications.
Smart Images

Figure BDA0004565694850000021 
Figure BDA0004565694850000023 
Figure BDA0004565694850000051
Abstract
Description
Technical Field
[0001] This invention belongs to the field of gas separation membranes, specifically relating to a gas separation membrane containing a sulfonate crosslinking structure and a blended polyimide hollow fiber and its preparation method. Background Technology
[0002] Polyimide is heat-resistant, chemically stable, and has high mechanical strength. Crucially, it possesses excellent gas separation performance, making it one of the ideal materials for gas separation membranes. Many researchers have dedicated themselves to studying the intrinsic gas separation properties of polyimide materials. Patents such as CN201210527698, CN201510249582, and CN201610495759 disclose the intrinsic gas separation properties of polyimides with specific molecular structures.
[0003] In practical applications such as natural gas / associated gas decarbonization, flue gas capture, and biogas recovery, flat-sheet or hollow fiber asymmetric gas separation membranes are typically used to improve the gas handling capacity of membrane modules. Studies have shown that the thinner the separation layer, the lower the membrane's resistance to CO2 plasticization, which places higher demands on the CO2 plasticization resistance of polyimide hollow fiber gas separation membrane materials. Furthermore, natural gas / associated gas, flue gas, and biogas often contain heavy hydrocarbons, water, and trace impurities. Heavy hydrocarbons, in particular, have a significant plasticizing / swelling effect on aromatic polyimides, thus affecting the membrane's gas separation performance.
[0004] Polymer crosslinking is considered an effective means to improve the anti-plasticization properties of membranes, but post-crosslinking treatment usually leads to a decrease in the membrane gas permeability coefficient. Known crosslinking methods mainly include decarboxylation thermal crosslinking, thermal oxidative crosslinking, diamine / diol / azide small molecule crosslinking, and high-temperature thermal rearrangement. Among these, diamine / diol / azide small molecule crosslinking requires crosslinking after the membrane material has been polymerized and molded, necessitating secondary processing. Furthermore, because asymmetric membranes have a denser skin, diamine / diol / azide small molecules cannot achieve 100% crosslinking of hollow fiber gas separation membranes; the crosslinking degree generally does not exceed 50%. Decarboxylation thermal crosslinking and high-temperature thermal rearrangement processes are relatively simple, but the processing temperature is usually above the glass transition temperature (Tg). This process has little impact on the gas separation performance of flat sheet dense membranes, but for asymmetric microporous membranes, heat treatment temperatures exceeding the glass transition temperature can cause the membrane micropores to collapse, thereby reducing the membrane flux and selectivity. Developing a technology that allows for excellent intrinsic gas permeation separation performance and enables crosslinking during the hollow fiber membrane module preparation process would be of great significance for gas separation membrane materials. Summary of the Invention
[0005] To address the above-mentioned issues, this invention provides a hollow fiber gas separation membrane with a sulfonate crosslinking structure and a blended polyimide, along with its preparation method. Two polyimides with different molecular structures and high gas flux are synthesized: one polyimide has highly rigid chain segments and hydroxyl functional groups on its side groups, while the other has highly flexible chain segments containing macromolecular side groups and sulfonic acid functional groups. The two polymers are blended, and a hollow fiber membrane module is prepared using a solvent-free phase inversion method. The membrane module undergoes an esterification crosslinking reaction in a vacuum environment at a high temperature below the glass transition temperatures of the two polymers to obtain a hollow fiber gas separation membrane with high mechanical strength, high flux, and resistance to plasticization.
[0006] This invention provides a sulfonate-crosslinked, blended polyimide hollow fiber gas separation membrane. The membrane comprises two polyimides: polyimide 1 and polyimide 2. The membrane is prepared by blending polyimide 1 and polyimide 2 in a molar ratio of 1:1 to 1:2 to obtain a hollow fiber membrane spinning solution. This solution is extruded through a hollow fiber nozzle and undergoes phase transformation in a coagulation bath to form a pre-formed polyimide hollow fiber membrane. After washing, drying, and winding, a membrane module is obtained, which is then subjected to thermal crosslinking. The thermal crosslinking temperature is 200–400°C, and is 20°C lower than the polymer's glass transition temperature.
[0007] The general structural formula of the polyimide 1 is:
[0008]
[0009] Where Ar is One of them;
[0010] The general structural formula of the polyimide 2 is:
[0011]
[0012] Where M is One of them;
[0013] Where J is
[0014] The molar ratio of M to J is 1:1.
[0015] This invention also provides a method for preparing a sulfonate crosslinked structure, blended polyimide hollow fiber gas separation membrane, comprising the following steps:
[0016] (1) Polyimide 1 and polyimide 2 were blended with solvent and non-solvent to prepare a hollow fiber membrane spinning solution;
[0017] The molar ratio of polyimide 1 to polyimide 2 is 1:1 to 1:2;
[0018] The solvent is one of NMP, DMAc, DMF, DMSO, and THF;
[0019] The non-solvent is one or two of water, methanol, ethanol, propanol, propionic acid, and butyric acid;
[0020] The solid content of the hollow fiber membrane spinning solution is 20-35 wt%.
[0021] (2) The hollow fiber membrane spinning solution is extruded through a hollow fiber nozzle and phase-transformed into a pre-formed polyimide hollow fiber membrane in a coagulation bath.
[0022] The coagulation bath is composed of one or two of the following: water, methanol, ethanol, and propanol.
[0023] (3) The initial polyimide hollow fiber membrane is washed in deionized water, then dried online by forced air drying, and the membrane is wound up to obtain a membrane module;
[0024] The cleaning time is 10–60 minutes;
[0025] The cleaning temperature is room temperature to 80°C;
[0026] The drying time is 10–60 min;
[0027] The drying temperature is room temperature to 100℃;
[0028] The film winding speed is 15-35 m / min.
[0029] (4) The membrane module is heated and crosslinked to obtain a gas separation membrane containing an acidic ester crosslinked structure and a blended polyimide hollow fiber structure;
[0030] The heating crosslinking temperature is 200-400°C, and the heating crosslinking temperature is 20°C lower than the polymer glass transition temperature.
[0031] The heating crosslinking atmosphere is one of nitrogen, argon, and helium;
[0032] The vacuum degree of the heating crosslinking is 0-50 kPa;
[0033] The heating crosslinking time is 10–24 h;
[0034] According to the invention, the hollow fiber gas separation membrane has a CO2 permeation flux of not less than 150 GPU and a CO2 plasticizing pressure resistance of not less than 3500 kPa.
[0035] The beneficial effects of this invention are as follows:
[0036] 1. The acid ester crosslinked structure, blended polyimide hollow fiber gas separation membrane is made by blending polyimide 1 with rigid chain and polyimide 2 with flexible chain, so that the two polyimides are highly miscible and the uniformity of the blend membrane is ensured.
[0037] 2. The rigid chain polyimide 1 carries hydroxyl groups, and the flexible chain polyimide 2 carries acidic functional groups, so that there are uniformly distributed crosslinking sites between polyimide 1 and 2.
[0038] 3. The crosslinking process of the membrane module is simple and the conditions are mild, and the microporous structure of the hollow fiber membrane remains stable during the crosslinking process;
[0039] 4. Through polyimide blending and crosslinking, a fixed microporous environment is formed between the polyimide chains, which maintains the stability of the membrane's free volume and gives the membrane material a high resistance to plasticization.
[0040] In summary, this invention prepares hollow fiber gas separation membranes through phase inversion by blending polymers with hydroxyl and acid functional groups, and then prepares high gas permeation flux and anti-plasticization hollow fiber gas separation membranes through a mild heating crosslinking process, thus solving the problem of membrane material stability in practical applications. Attached Figure Description
[0041] Figure 1 Scanning electron microscope (SEM) image of a hollow fiber gas separation membrane containing an acidic ester crosslinking structure and blended polyimide, prepared according to the present invention, after 360°C crosslinking heat treatment. Detailed Implementation
[0042] The present invention will be described below through specific embodiments, but the present invention is not limited thereto.
[0043] Unless otherwise specified, the experimental methods used in the following examples are conventional methods; unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0044] Example 1:
[0045] Polyimide 1: Solid polyimide 1 was prepared by low-temperature polymerization of 1 mol of 2,2'-dihydroxybenzyldiamine (HAB) and 1 mol of naphthyltetracarboxylic anhydride (NTDA). The glass transition temperature of polyimide 1 was tested to be 416℃.
[0046] Polyimide 2: Polymerization of 0.5 mol diaminobenzenesulfonic acid (DAS) and 0.5 mol tetramethylphenylenediamine (DAM) with 1 mol hexafluorodianhydride (6FDA) yielded solid polyimide 2. The glass transition temperature of polyimide 2 was tested to be 395 °C.
[0047] Preparation of membrane forming slurry: 150g of polyimide 1 is blended with 400g of DMAc and heated and stirred at 80°C to form polyimide 1 slurry; 300g of polyimide 2 is blended with 800g of DMAc and heated and stirred at 80°C to form polyimide 2 slurry; polyimide 1 slurry and polyimide 2 slurry are blended together, and 75g of methanol is added, and stirring is continued to form hollow fiber membrane spinning solution.
[0048] Hollow fiber gas separation membrane module forming: The hollow fiber membrane spinning solution is delivered to the hollow fiber membrane spinneret by a gear pump, and a preliminary polyimide hollow fiber membrane is formed in a water coagulation bath. The preliminary polyimide hollow fiber membrane is then thoroughly washed with water at 40°C for 20 minutes to remove the solvent from the membrane fibers; it continues to enter the forced-air drying oven and is heated and dried at 120°C for 5 minutes; then the membrane is wound up at a winding speed of 20 m / min to obtain membrane module 1.
[0049] Hollow fiber gas separation membrane heating crosslinking: Membrane module 1 is slowly heated to a certain temperature in a nitrogen atmosphere, with temperatures of 300, 320, 340, 360, 380, and 400℃ respectively, while maintaining a nitrogen flow rate of not less than 30 m / min and maintaining the heating time for 2 hours, so that an ester crosslinking network structure is formed between the polymer chains of the hollow fiber gas separation membrane, resulting in hollow fiber gas separation membranes 2, 3, 4, 5, 6, and 7 containing acidic ester crosslinking structure and blended polyimide.
[0050] The separation performance and CO2 plasticizing resistance of gas separation membranes with different crosslinking temperatures, containing acidic ester crosslinking structures, and blended polyimide hollow fiber membranes were compared. The results are as follows:
[0051]
[0052] Example 2:
[0053] The molecular structures of polyimide 1 and polyimide 2 are the same as those in Example 1.
[0054] Preparation of membrane forming slurry: 200g of polyimide 1 is blended with 570g of DMAc and heated and stirred at 80℃ to form polyimide 1 slurry; 300g of polyimide 2 is blended with 800g of DMAc and heated and stirred at 80℃ to form polyimide 2 slurry; polyimide 1 slurry and polyimide 2 slurry are blended together, and 85g of methanol is added, and stirring is continued to form hollow fiber membrane spinning solution.
[0055] Hollow fiber gas separation membrane module molding: The process is the same as in Example 1, resulting in membrane module 8.
[0056] Hollow fiber gas separation membrane heating crosslinking: Membrane module 8 is slowly heated to a certain temperature in a nitrogen atmosphere, with temperatures of 360, 380, and 400℃ respectively, while maintaining a nitrogen flow rate of not less than 30 m / min and maintaining the heating time for 2 hours, so that an ester crosslinking network structure is formed between the polymer chains of the hollow fiber gas separation membrane, resulting in hollow fiber gas separation membranes 9, 10, and 11 containing acidic ester crosslinking structure and blended polyimide.
[0057] The gas separation performance and CO2 plasticizing resistance of polyimide hollow fiber gas separation membranes with different crosslinking temperatures and acidic ester crosslinking structures were compared. The results are as follows:
[0058]
[0059] Example 3:
[0060] The molecular structures of polyimide 1 and polyimide 2 are the same as those in Example 1.
[0061] Preparation of membrane forming slurry: 300g of polyimide 1 and 800g of DMAc are blended and heated at 80°C with stirring to dissolve and form polyimide 1 slurry; 300g of polyimide 2 and 800g of DMAc are blended and heated at 80°C with stirring to dissolve and form polyimide 2 slurry; polyimide 1 slurry and polyimide 2 slurry are blended together, and 100g of methanol is added, and stirring is continued to form hollow fiber membrane spinning solution.
[0062] Hollow fiber gas separation membrane module molding: The process is the same as in Example 1, resulting in membrane module 12.
[0063] Hollow fiber gas separation membrane heating crosslinking: Membrane module 12 is slowly heated to a certain temperature in a nitrogen atmosphere, the temperatures being 360, 380, and 400℃ respectively, while maintaining a nitrogen flow rate of not less than 30 m / min and maintaining the heating time for 2 hours, so that an ester crosslinking network structure is formed between the polymer chains of the hollow fiber gas separation membrane, resulting in hollow fiber gas separation membranes 13, 14, and 15 containing acidic ester crosslinking structure and blended polyimide.
[0064] The gas separation performance and CO2 plasticizing resistance of polyimide hollow fiber gas separation membranes with different crosslinking temperatures and acidic ester crosslinking structures were compared. The results are as follows:
[0065]
[0066]
[0067] Comparative example:
[0068] Polyimide: Polyimide A solid was obtained by polymerizing 0.5 mol of 2,6-diaminotoluene and 0.5 mol of tetramethylphenylenediamine (DAM) with 1 mol of 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA). The glass transition temperature of the polyimide was tested to be 387℃.
[0069] Preparation of membrane forming slurry: 300g of polyimide A and 800g of DMAc are mixed, heated and stirred at 80℃ to dissolve, then 75g of methanol is added and stirring is continued to form hollow fiber membrane spinning solution.
[0070] Hollow fiber gas separation membrane module forming: The hollow fiber membrane spinning solution is pumped to the hollow fiber membrane spinneret via a gear pump, forming a preliminary polyimide hollow fiber membrane in a water coagulation bath. The preliminary polyimide hollow fiber membrane is then thoroughly washed with water at 40°C for 20 minutes to remove the solvent from the membrane fibers; it is then further placed in a forced-air drying oven and heated to 120°C for 5 minutes; finally, the membrane is wound up at a winding speed of 20 m / min to obtain Comparative Example-Membrane 1. Hollow fiber gas separation membrane thermal crosslinking: Comparative Example-Membrane 1 is slowly heated to 360°C in a nitrogen atmosphere, maintaining a nitrogen flow rate of no less than 30 m / min, and maintained for 2 hours to obtain Comparative Example-Membrane 2.
[0071]
[0072] The above embodiments are only for illustrating the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.
[0073] Matters not covered in this invention are common knowledge.
Claims
1. A gas separation membrane containing an acidic ester crosslinking structure and a blend of polyimide hollow fibers, characterized in that, The acid ester crosslinked structure, blended polyimide hollow fiber gas separation membrane comprises polyimide 1 and polyimide 2. The acid ester crosslinked structure, blended polyimide hollow fiber gas separation membrane is prepared by blending polyimide 1 and polyimide 2 in a molar ratio of 1:1 to 1:2 to obtain a hollow fiber membrane spinning solution. The hollow fiber membrane spinning solution is extruded through a hollow fiber nozzle and undergoes phase transformation in a coagulation bath to form a preliminary polyimide hollow fiber membrane. After washing, drying, and winding, a membrane module is obtained, which is then subjected to heating crosslinking to obtain the final product. The heating crosslinking temperature is 200–400°C, and is 20°C lower than the polymer's glass transition temperature. The general structural formula of the polyimide 1 is: Where Ar is One of them; The general structural formula of the polyimide 2 is: Where M is One of them; Where J is The molar ratio of M to J is 1:
1.
2. A method for preparing the gas separation membrane containing an acidic ester crosslinking structure and blended polyimide hollow fiber as described in claim 1, characterized in that, Includes the following steps: (1) Polyimide 1 and polyimide 2 are blended with solvent and non-solvent to prepare a hollow fiber membrane spinning solution; the molar ratio of polyimide 1 and polyimide 2 is 1:1 to 1:2; The solvent is one of NMP, DMAc, DMF, DMSO, and THF; The non-solvent is one or two of water, methanol, ethanol, propanol, propionic acid, and butyric acid; The solid content of the spinning solution for the hollow fiber membrane is 20-35 wt%. (2) The hollow fiber membrane spinning solution is extruded through a hollow fiber nozzle and phase-transformed into a pre-formed polyimide hollow fiber membrane in a coagulation bath. (3) The initial polyimide hollow fiber membrane is washed in deionized water, then dried online by forced air drying, and the membrane is wound up to obtain a membrane module; (4) The membrane module is heated and crosslinked to obtain a gas separation membrane containing an acidic ester crosslinked structure and a blended polyimide hollow fiber structure; The heating crosslinking temperature is 200-400°C, and the heating crosslinking temperature is 20°C lower than the polymer glass transition temperature. The heating crosslinking atmosphere is one of nitrogen, argon, and helium; The vacuum degree of the heating crosslinking is 0-50 kPa; The heating crosslinking time is 10–24 h.
3. The method for preparing a hollow fiber gas separation membrane containing an acidic ester crosslinking structure and blended polyimide according to claim 2, characterized in that, The coagulation bath in step (2) consists of one or two of water, methanol, ethanol, and propanol.
4. The method for preparing a gas separation membrane containing an acidic ester crosslinking structure and blended polyimide hollow fiber according to claim 2, characterized in that, The cleaning time in step (3) is 10 to 60 minutes; the cleaning temperature is room temperature to 80°C.
5. The method for preparing a gas separation membrane containing an acidic ester crosslinking structure and blended polyimide hollow fiber according to claim 2, characterized in that, The drying time in step (3) is 10 to 60 minutes; the drying temperature is room temperature to 100°C.
6. The method for preparing a gas separation membrane containing an acidic ester crosslinking structure and blended polyimide hollow fiber according to claim 2, characterized in that, The film winding speed in step (3) is 15-35 m / min.
Citation Information
Patent Citations
Copolymerization polyimide gas separation membrane material, preparation method and application of copolymerization polyimide gas separation membrane material
CN103846023A
Polyimide gas separation membrane as well as preparation method and applications thereof
CN104829853A
Polyimide gas separation membrane and preparation method and application thereof
CN106139936A
All-polyimide mixed matrix gas separation membrane and preparation method and application thereof
CN112354381A
Polyimide pervaporation separation membrane and preparation method and separation method thereof
CN112705050A