Laser cladding manufacturing method for thread rolling wheel
By using 40Mn2 steel on the rolling wheel and performing laser cladding alloy layer and stress relief annealing treatment, the problems of high brittleness and poor welding performance of the rolling wheel are solved, high hardness and wear resistance are achieved, and the repair process is extended service life, reducing production costs and resource waste.
Patent Information
- Application Number
- CN202311432262.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-10-31
AI Technical Summary
In the production process of existing rolling wheels, the cold work die steel has high hardness but is brittle, easy to collapse, has poor welding performance, and the vacuum heat treatment cost is high and difficult to repair, resulting in a waste of resources.
Using 40Mn2 steel as the base of the rolling wheel, laser cladding the alloy layer and performing stress relief annealing treatment, combined with mechanical processing, forms a rolling wheel with high hardness, wear resistance and excellent welding performance, and goes through the same steps after wear Make repairs.
It achieves high hardness, wear resistance and good welding performance of the rolling wheel, reduces production costs, extends service life, and saves rare metal resources.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of laser cladding, and in particular to a laser cladding manufacturing method for a thread rolling wheel. Background Art
[0002] A thread rolling wheel is a tool that uses the method of metal plastic deformation to roll out threads on a thread rolling machine.
[0003] At present, thread rolling wheels are usually made of cold working die steel such as Cr12MoV or DC53. The surface is reverse rolled and then vacuum quenched to increase the surface hardness to above HRC60. The thread rolling wheels made by the above process can meet daily production needs, but there are the following problems:
[0004] (1) The carbon and alloy element content in cold working die steel is high. Although the hardness is very high after heat treatment, its plasticity and toughness are low, and thread collapse often occurs during use.
[0005] (2) The carbon content and alloy content of cold working die steel are high, and the material welding performance is poor; it is difficult to perform welding repair after wear and thread breakage.
[0006] (3) The heat treatment process during the manufacturing process requires vacuum quenching, which is a complex process with high cost.
[0007] (4) Cold working die steel contains rare and precious alloy elements, and scrapping the thread rolling wheel will waste such resources. Summary of the invention
[0008] In view of the problems of high vacuum heat treatment cost, high material brittleness, easy collapse, poor welding performance, and difficulty in repair during the production and use of thread rolling wheels, the present invention provides a laser cladding manufacturing method for thread rolling wheels. The prepared thread rolling wheels have the advantages of high hardness, strong wear resistance, excellent welding performance, and easy repair, while having low production cost.
[0009] The present invention provides a laser cladding manufacturing method for a thread rolling wheel, comprising the following steps:
[0010] S1. The base material of the thread rolling wheel is 40Mn2 steel;
[0011] S2, laser cladding alloy layer on the surface of the thread rolling wheel substrate;
[0012] S3, stress relief annealing treatment of the thread rolling wheel substrate after laser cladding;
[0013] S4. The thread surface is obtained by machining the thread rolling wheel base.
[0014] Furthermore, in step S1, the thread rolling wheel substrate is obtained by forging and tempering 40Mn2 steel. The thread rolling wheel substrate has a tensile strength of 885MPa and a yield strength of 735MPa, and the strength can meet the requirements of the workpiece.
[0015] Furthermore, in step S2, the surface of the thread rolling wheel substrate is pretreated before laser cladding, and the pretreatment method is turning the surface of the thread rolling wheel substrate. After turning, the working surface diameter of the thread rolling wheel substrate is 4-5 mm shorter than the finished product size diameter, which is used to reserve the thickness of the laser cladding alloy layer.
[0016] Furthermore, in step S2, the method for laser cladding the alloy layer on the surface of the wire wheel substrate is to clad the alloy powder onto the surface of the wire wheel substrate through a laser cladding process.
[0017] Furthermore, the laser cladding process parameters are as follows: cladding power of 5000~6000W, spot size of 20*2mm, cladding line speed of 300~500mm / min, overlap rate of 50%~60%, and cladding layer thickness of 2.5~3mm.
[0018] Furthermore, the alloy powder has a particle size of 100~400 meshes, and the alloy powder includes the following weight percentages: C0.015%~0.02%, Mn 0.25%~0.35%, B 1.1%~1.2%, Si 1.1%~1.2%, Cr 14.5%~15.5%, Ni 1.5%~1.8%, Mo 1.0%~1.2%, and the rest is Fe and other trace impurities. The carbon content in its composition is low, and the material has good welding performance. The boron, silicon and manganese elements in its composition play a reinforcing role to improve its strength, hardness and wear resistance. The chromium and nickel elements in the composition can make the cladding layer have better intergranular corrosion resistance, improve its strength and corrosion resistance. The molybdenum element can reduce the temper brittleness of the workpiece when it is kept at about 250°C, so that the cladding layer has good plasticity and toughness, and avoids thread collapse during use. After cladding, the alloy powder can obtain fine hidden martensite and bainite structures, and its hardness after cladding can reach HRC60.
[0019] Furthermore, in step S3, the method for stress relief annealing of the thread rolling wheel substrate is that after laser cladding, the thread rolling wheel substrate is placed in a heat treatment furnace at a temperature of 200-250° C. while hot for 2-3 hours, and then buried in insulation sand and slowly cooled.
[0020] Furthermore, in step S4, a CNC lathe is used to machine the surface of the thread rolling wheel substrate using a boron nitride turning tool to complete thread processing and forming.
[0021] Furthermore, in step S4, the thread rolling wheel substrate is subjected to demagnetization treatment after mechanical processing.
[0022] The present invention is also applicable to repairing the thread rolling wheel made by the present invention after it is worn or otherwise damaged. Specifically, the repair process can be performed by executing the above-mentioned steps S2-S4, and the repaired base can be used repeatedly.
[0023] The beneficial effects of the present invention are as follows: the thread rolling wheel manufactured by the present invention solves the problems of high vacuum heat treatment cost, high material brittleness, easy collapse, poor welding performance, and difficulty in repair during the production and use of existing thread rolling wheels. At the same time, the production cost can be saved by replacing the base material. It also has the social benefit of saving rare and precious metals. DETAILED DESCRIPTION
[0024] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0025] Example 1
[0026] A Shanghai company newly manufactured a 54-type 20 series standard thread rolling wheel. The process flow of its laser cladding manufacturing method is as follows:
[0027] (1) The thread rolling wheel base is made of 40Mn2 steel forging and tempering treatment.
[0028] (2) The surface of the thread rolling wheel base is turned to a diameter of 145 mm. After turning, the working surface diameter of the thread rolling wheel base is 4 to 5 mm shorter than the finished product diameter.
[0029] (3) Prepare laser cladding powder. The cladding layer should have the characteristics of impact resistance and wear resistance. The chemical composition of the alloy powder is as follows: carbon 0.02%, manganese 0.3%, boron 1.2%, silicon 1.15%, chromium 15%, nickel 1.7%, molybdenum 1.0%, and the rest is iron and other trace impurities. The powder size range is 100-270 mesh. The powder is fully mixed and dried before use.
[0030] (4) Formulate a reasonable laser cladding process for laser cladding, and its process parameters are: cladding power P = 6000W, spot size B = 20*2mm, cladding line speed V = 380mm / min, overlap rate 50%, and cladding layer thickness 3mm.
[0031] (5) After laser cladding, the material is placed in a heat treatment furnace at 250°C while hot and kept warm for 2 hours. Then, it is buried in insulating sand and slowly cooled to complete the stress relief annealing process.
[0032] (6) Use a CNC lathe and a boron nitride turning tool to machine the surface of the thread rolling wheel to complete the thread machining.
[0033] (7) Demagnetization treatment.
[0034] The 54-type 20 series thread rolling wheel produced in this example was sampled and tested, and its hardness reached HRC62, and the cladding layer was fine hidden martensite and bainite structure. The online trial tracking lasted for 1000 hours without damage, and the final service life was more than doubled.
[0035] Example 2
[0036] A company in Shanghai laser manufactures 54-type 20 series standard thread rolling wheels for repair after wear, and the method of the present invention is also applicable. The process flow is as follows:
[0037] (1) The damaged thread rolling wheel substrate (the thread rolling wheel substrate is obtained by forging and tempering 40Mn2 steel) is surface turned and the diameter is turned to 145 mm. After turning, the working surface diameter of the thread rolling wheel substrate is 4-5 mm shorter than the finished product diameter.
[0038] (2) Prepare laser cladding powder. The cladding layer should have the characteristics of impact resistance and wear resistance. The chemical composition of the alloy powder is as follows: carbon 0.018%, manganese 0.32%, boron 1.2%, silicon 1.1%, chromium 14.8%, nickel 1.6%, molybdenum 1.1%, and the rest is iron and other trace impurities. The powder size range is 270-400 mesh. The powder is fully mixed and dried before use.
[0039] (3) Formulate a reasonable laser cladding process for laser cladding, and its process parameters are: cladding power P = 5800W, spot size B = 20*2mm, cladding line speed V = 400mm / min, overlap rate 50%, and cladding layer thickness 3mm.
[0040] (4) After laser cladding, the material is placed in a heat treatment furnace at 220°C while hot and kept warm for 3 hours. The material is then buried in insulating sand and slowly cooled to complete the stress relief annealing process.
[0041] (5) Use a CNC lathe and a boron nitride turning tool to machine the surface of the thread rolling wheel to complete the thread machining.
[0042] (6) Demagnetization treatment.
[0043] This example is an example of repairing a damaged laser-made thread rolling wheel. The repaired thread rolling wheel has the same performance and service life as a new laser thread rolling wheel, making the thread rolling wheel repair possible.
[0044] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and such modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily conceive of changes or substitutions within the technical scope disclosed by the present invention, and such changes or substitutions shall be within the scope of protection of the present invention.
Claims
1. A laser cladding manufacturing method for a thread rolling wheel, characterized in that: The steps include: S1. The base material of the thread rolling wheel is 40Mn2 steel; S2, laser cladding alloy layer on the surface of the thread rolling wheel substrate; S3, stress relief annealing treatment of the thread rolling wheel substrate after laser cladding; S4, machining the thread rolling wheel base to obtain the thread surface; In step S2, the method for laser cladding the alloy layer on the surface of the wire wheel substrate is to clad the alloy powder onto the surface of the wire wheel substrate through a laser cladding process, and the laser cladding process parameters are: cladding power of 5000-6000 W, spot size of 20*2 mm, cladding line speed of 300-500 mm / min, overlap rate of 50%-60%, cladding layer thickness of 2.5-3 mm, and the alloy powder includes the following components in weight percentage: C 0.015%-0.02%, Mn 0.25%-0.35%, B 1.1%-1.2%, Si 1.1%-1.2%, Cr14.5%-15.5%, Ni 1.5%-1.8%, Mo 1.0%-1.2%, and the rest is Fe and other trace impurities; In step S3, the method for stress relief annealing of the thread rolling wheel substrate is that after laser cladding, the thread rolling wheel substrate is placed in a heat treatment furnace at a temperature of 200-250° C. while hot for 2-3 hours, and then buried in insulation sand to cool slowly; In step S4, a CNC lathe is used to machine the surface of the thread rolling wheel substrate using a boron nitride turning tool to complete thread processing and forming.
2. The laser cladding manufacturing method of the thread rolling wheel according to claim 1, characterized in that: In step S1, the thread rolling wheel substrate is obtained by forging and tempering 40Mn2 steel.
3. The laser cladding manufacturing method of a thread rolling wheel according to claim 1, characterized in that: In step S2, the surface of the thread rolling wheel substrate is pretreated before laser cladding. The pretreatment method is turning the surface of the thread rolling wheel substrate. After turning, the working surface diameter of the thread rolling wheel substrate is 4-5 mm shorter than the finished product size diameter.
4. The laser cladding manufacturing method of a thread rolling wheel according to claim 1, characterized in that: The particle size of the alloy powder is 100~400 mesh.
5. The laser cladding manufacturing method of a thread rolling wheel according to claim 1, characterized in that: In step S4, the thread rolling wheel substrate is subjected to demagnetization treatment after machining.
Citation Information
Patent Citations
High hardness material laser cladding process method for roller work surface
CN103255412A
Metal powder for repairing foot roller of continuous casting crystallizer through laser cladding and preparation method of metal powder
CN113789469A