Metallic lithium negative electrode of "sandwich" structure and method of preparation and use thereof
By using a 'sandwich' structure for the lithium metal anode, the problems of lithium dendrite formation and volume expansion are solved, improving the cycle life and safety of lithium batteries and enhancing ion transport speed.
Patent Information
- Application Number
- CN202210953081.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-04
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-08-04
AI Technical Summary
During charging and discharging, lithium metal anodes expand in volume, causing the SEI layer to crack and lithium dendrites to form, which leads to safety issues. Existing three-dimensional carbon materials have not been able to completely solve the lithium dendrite problem.
The lithium metal anode adopts a 'sandwich' structure, with a lithiophilic carbonized fiber film at the bottom, an ultrathin lithium strip in the middle, and an uncarbonized fiber film at the top. Lithophilic seed sites are formed through cross-linking and carbonization treatment, and conductive and non-conductive layers are designed to guide the directional deposition of lithium ions.
It effectively accommodates lithium volume expansion, reduces lithium dendrite formation, improves battery cycle life and safety, and enhances ion transport speed.
Smart Images

Figure CN117558867B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of energy storage technology, and in particular to a lithium metal anode that can be used in secondary batteries, its preparation method, and its application. Background Technology
[0002] Lithium metal anodes are valued for their high theoretical capacity (3860 mAh / g), lowest reduction potential (-3.04 V, relative to standard hydrogen potential), and low density (0.534 g / cm³). 3 Lithium metal is an ideal material for next-generation high-energy-density batteries. However, due to the lack of a host cell and the high reactivity of lithium metal, the volume of the lithium metal anode expands during battery charging and discharging, leading to the rupture of the solid electrolyte interphase (SEI) layer. This causes continuous side reactions between lithium metal and the electrolyte, resulting in the loss of active lithium. + Uneven deposition of lithium dendrites can easily lead to the formation of lithium dendrites, which can puncture the separator, causing short circuits in the battery and even safety issues such as fires and explosions. Three-dimensional carbon materials can effectively alleviate the volume expansion problem of lithium metal anodes, but the problem of lithium dendrites still exists. Summary of the Invention
[0003] To address the aforementioned issues, the inventors of this application have developed a "sandwich" structure for lithium metal anodes. Its spatial structure can accommodate lithium metal to alleviate volume expansion, with the bottom layer being conductive and the top layer being non-conductive, which can guide the directional deposition of lithium ions in the bottom layer, thereby improving the cycle life and safety of lithium metal batteries.
[0004] To achieve the above objectives, the present invention adopts the following technical solution:
[0005] According to one aspect of the present invention, a "sandwich" structured lithium metal anode is provided, the lithium metal anode comprising:
[0006] As the underlying lithium-loving carbon fiber membrane material,
[0007] The ultra-thin lithium strip as the intermediate layer, and
[0008] As the top layer of uncarbonized fiber membrane material,
[0009] The lithium-loving carbonized fiber membrane is formed by carbonizing a cross-linked three-dimensional fiber network and then growing nanoscale lithium-loving seed sites on the surface of the fiber filaments.
[0010] The thickness of the ultrathin lithium strip is less than 100 μm (e.g., 1-100 μm, preferably 10-80 μm).
[0011] The uncarbonized fiber membrane material is a cross-linked three-dimensional fiber network that has not undergone carbonization treatment.
[0012] The thickness of the lithium metal anode is in the range of 80-180 μm.
[0013] In some embodiments, the bottom layer has conductive lithium-philic properties, and the top layer is a porous, non-conductive layer.
[0014] In some embodiments, the three-dimensional fiber network is formed by electrospinning and crosslinking of polyacrylonitrile and / or polyimide, with the crosslinking of the fibers occurring during the electrospinning film formation process.
[0015] In some embodiments, the lithiophilic seed sites are formed by impregnating the carbonized fiber membrane with a metal salt solution, drying it, and then using microwave heating to provide a heat source to reduce the metal ions.
[0016] According to another aspect of the present invention, a method for preparing the above-described "sandwich" structured lithium metal anode is provided, the method comprising:
[0017] Electrospinning of polyacrylonitrile and / or polyimide, cross-linking treatment during the formation of fiber membrane, and collection of the spun fiber membrane;
[0018] The cross-linked fiber membrane is carbonized, the carbonized fiber membrane is impregnated with a metal salt solution, the impregnated fiber membrane is dried, and then microwave heating is performed to reduce it, so as to obtain a carbonized fiber membrane with lithium affinity.
[0019] Using the lithium-loving carbonized fiber membrane as the bottom layer, the ultra-thin lithium strip as the middle layer, and the uncarbonized cross-linked fiber membrane as the top layer, the three layers are rolled together using a roller press.
[0020] In some embodiments, the electrospinning solution comprises: dissolving polyacrylonitrile and / or polyimide in dimethylformamide or N-methylpyrrolidone to prepare a precursor solution with a concentration of 5-15 wt%, preferably 7 wt%; applying a high voltage of 8-15 kV, preferably 8-10 kV (distance: about 14 cm) between needles and aluminum foil on a rotating drum; electrospinning the precursor solution at a rate of 0.4-3 mL / h, preferably 1-3 mL / h; and collecting the spun fiber membrane.
[0021] In some embodiments, the crosslinking process involves placing ultraviolet lamps on both sides in front of the electrospinning nozzle to crosslink the fibers by irradiation with ultraviolet light.
[0022] In some embodiments, the ultraviolet light source is a 2-5kW mercury lamp irradiation, the temperature is 50-80°C, preferably 70°C, and the irradiation time is 20-50 minutes, preferably 30 minutes.
[0023] In some embodiments, the cross-linked fiber membrane after electrospinning satisfies at least one of the following conditions:
[0024] The transverse and / or longitudinal breaking strength is 12-40N, preferably 20-40N;
[0025] The thickness is 25-60μm, preferably 60μm.
[0026] In some embodiments, the carbonization process includes:
[0027] The fiber membrane is calcined in air at 200-360°C, preferably 240-300°C, for 2-4 hours, preferably 2-3 hours, and then calcined in an inert gas at 700-1200°C, preferably 1100-1200°C, for 3-6 hours, preferably 2-4 hours.
[0028] In some embodiments, the carbonized fiber membrane material impregnated with a metal salt solution includes:
[0029] The fiber membrane material is immersed in a salt solution of silver, zinc, gold or magnesium, preferably subjected to 3-8 vacuum filtrations.
[0030] The soaked fiber membrane is dried at 40-100℃, preferably 60-80℃.
[0031] In some embodiments, the microwave heating reduction includes:
[0032] Heating at a microwave frequency of 2400-3000MHz and a power of 700-900W for 10-60s, preferably 10-30s, generates in-situ lithium-affinity seed sites on the fiber membrane.
[0033] In some embodiments, the thickness of the ultrathin lithium strip is 20-100 μm.
[0034] In some implementations, the roller press pressure is 5-10 MPa, preferably 8 MPa.
[0035] In some implementations, the thickness of the rolled “sandwich” structured lithium metal anode is in the range of 80-180 μm.
[0036] According to another aspect of the present invention, the application of the above-described "sandwich" structured lithium metal anode in a lithium metal battery is provided.
[0037] In some embodiments, the lithium metal battery includes a lithium metal secondary battery.
[0038] According to the technical solution of the present invention, the following beneficial effects can be provided:
[0039] The "sandwich" structure lithium metal anode of this invention has a three-dimensional spatial structure that can accommodate the volume expansion of lithium metal. Furthermore, the unique design of a lithium-philic and conductive bottom layer and a non-conductive top layer guides the directional deposition of lithium in the bottom layer, significantly mitigating lithium dendrite growth and improving the cycle life and safety of lithium metal batteries. The porous structure of the top fiber membrane allows for better electrolyte permeation, increasing ion transport velocity. Therefore, the "sandwich" structure lithium metal anode has significant application value in the field of lithium metal rechargeable batteries. Attached Figure Description
[0040] Figure 1 This is a schematic diagram of the "sandwich" structure of the lithium metal anode of the present invention.
[0041] Figure 2 This is a schematic cross-sectional view of the "sandwich" structure of the lithium metal anode of the present invention.
[0042] Figure 3 These are electron micrographs of an uncrosslinked, uncarbonized fiber membrane (a); a crosslinked, uncarbonized fiber membrane (b); a crosslinked, carbonized fiber membrane (c); and a crosslinked, carbonized fiber membrane with lithium-loving seed sites (d).
[0043] Figure 4 This is a capacity test diagram of "sandwich" structured lithium metal anodes with different lithium strip thicknesses.
[0044] Figure 5 These are cycle test diagrams of "sandwich" structured lithium metal anodes with lithium strip thicknesses of 20 μm (a), 60 μm (b), and 100 μm (c).
[0045] Figure 6 This is a cyclic test diagram of Comparative Example 1 and Comparative Example 2. Detailed Implementation
[0046] The present invention will now be described in conjunction with the accompanying drawings and specific embodiments. However, it should be understood that the following specific embodiments are merely illustrative of implementation schemes of the present invention, and the scope of protection of the present invention is not limited thereto.
[0047] Example
[0048] Example 1
[0049] Polyacrylonitrile (Changzhou Tianyi Engineering Fiber Co., Ltd.) was dissolved in dimethylformamide (Aladdin Reagent Network) to prepare a 7wt% solution, which was used as the precursor solution for electrospinning. Two UV lamps (UV lamp model: GE.R 500W Helios Italquartz, 250-450nm, λ) were placed on either side of the electrospinning nozzle. max=360nm), the needle distance from the UV lamp was 1-3cm, then electrospinning began, the high-strength portion of the electrospun fiber membrane was collected and calcined in air at 240-300℃ for 2-4h, and then carbonized in an argon flow at 1100-1200℃ for 2-4h to obtain a carbonized fiber membrane. The carbonized fiber membrane was filtered 3-5 times with 0.05mol / L silver acetate (Aladdin reagent net), and then dried in an oven at 60-80℃ for 2h. The dried fiber membrane was heated in a microwave at 2600MHz and 700W for 10-15s to generate lithiophilic seed sites in situ on the fiber membrane material. Then, a 20μm ultrathin lithium strip (Tianjin Zhongneng Lithium Industry Co., Ltd.) was rolled onto the carbonized fiber membrane with lithium-loving seed sites. The uncarbonized fiber membrane was then covered on the ultrathin lithium strip and rolled on a roller press at a pressure of 8Mpa to obtain a "sandwich" structured lithium metal anode with a total thickness of 80μm.
[0050] Example 2
[0051] The main difference between this embodiment and Embodiment 1 is that the ultrathin lithium strip is 60μm and the total thickness of the lithium metal anode is 120μm.
[0052] Example 3
[0053] The main difference between this embodiment and Embodiment 1 is that the ultrathin lithium strip is 100μm and the total thickness of the metallic lithium anode is 180μm.
[0054] Example 4
[0055] The lithium metal anode from Example 1 was cut into electrode sheets with a diameter of 14 mm using a cutting machine; the lithium sheet was used as the counter electrode, and 1M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) (solvent: 1,3-dioxolane (DOL): ethylene glycol dimethyl ether (DME) volume ratio of 1:1, with 2wt% LiNO3 as an additive) was used as the electrolyte (Ningbo Shanshan Co., Ltd.), Cellgard 2000 Using a separator, 2025-type button cells were assembled and their capacity tested in a glove box (high-purity argon atmosphere, where O2 and H2O content are both less than 0.01 ppm). Then, symmetrical cells were assembled and their capacity tested at 3 mA / cm². 2 Current density and 3mAh / cm 2 The cycling performance of this lithium metal anode was tested at the areal capacity.
[0056] Example 5
[0057] The main difference between this embodiment and Embodiment 4 is that a cutting machine is used to cut the lithium metal anode from Embodiment 2 into electrode sheets with a diameter of 14 mm; the lithium sheet is used as the counter electrode to assemble a 2025 type button cell for capacity testing. Then, a symmetrical cell is assembled, and the capacity is tested at 3 mA / cm².2 Current density and 3mAh / cm 2 The cycling performance of this lithium metal anode was tested at the areal capacity.
[0058] Example 6
[0059] The main difference between this embodiment and Embodiment 4 is that the lithium metal anode from Embodiment 3 is cut into electrode sheets with a diameter of 14 mm using a cutting machine; the lithium sheet is used as the counter electrode to assemble a 2025 type button cell for capacity testing. Then, a symmetrical cell is assembled, and the capacity is tested at 3 mA / cm². 2 Current density and 3mAh / cm 2 The cycling performance of this lithium metal anode was tested at the areal capacity.
[0060] Comparative Example 1
[0061] Symmetrical cells were assembled using 20, 60, and 100 μm lithium wafers from Zhongneng Lithium Industry Co., Ltd., achieving an efficiency of 3 mA / cm². 2 Current density and 3mAh / cm 2 Cyclic performance was tested at areal capacity.
[0062] Comparative Example 2
[0063] Lithium metal anodes with structures of ungrown lithiophilic sites on a carbon fiber membrane + 60 μm ultrathin lithium strip + ungrown carbon fiber membrane and lithium metal anodes with grown lithiophilic sites on a carbon fiber membrane + 60 μm ultrathin lithium strip were prepared. The lithium metal anodes were cut into electrode sheets with a diameter of 14 mm using a cutting machine; 1M LiTFSI (solvent:DOL:DME volume ratio 1:1, 2wt% LiNO3 as additive) was used as the electrolyte, and Cellgard 2000 was used. Using a diaphragm, a 2025-type button cell was assembled in a glove box (high-purity argon atmosphere, where the O2 and H2O contents are both less than 0.01 ppm), at 3 mA / cm². 2 Current density and 3mAh / cm 2 The cycling performance of this lithium metal anode was tested at the areal capacity.
[0064] Table 1 compares the tensile strength of uncrosslinked and crosslinked / crosslinked carbonized fiber membranes. As can be seen from Table 1, the tensile strength of the crosslinked fiber membrane is significantly improved, and the strength of the fiber membrane does not decrease significantly after carbonization.
[0065] Table 1
[0066]
[0067] Figure 1 This is a schematic diagram of the "sandwich" structure of the lithium metal anode of the present invention; Figure 2This is a schematic cross-sectional view of the "sandwich" structure of the lithium metal anode of this invention. The bottom layer is a carbonized fiber film with lithiophilic sites, the middle layer is an ultrathin lithium strip, and the top layer is an uncarbonized fiber film.
[0068] Figure 3 These are electron micrographs of an uncrosslinked, uncarbonized fiber membrane (a); a crosslinked, uncarbonized fiber membrane (b); a crosslinked, carbonized fiber membrane (c); and a crosslinked, carbonized fiber membrane with long lithium-affinity seed sites (d). The figures show that crosslinking occurs between the fiber filaments after treatment, improving the tensile strength of the fiber membrane. After carbonization, the crosslinking status remains largely unchanged. In (d), lithium-affinity seed sites are uniformly distributed on the fiber filaments, enhancing the affinity of the fiber membrane for lithium.
[0069] Figure 4 This is a capacity test chart of "sandwich" structure lithium metal anodes with different lithium strip thicknesses. The chart shows that the capacity of the lithium metal anodes ranges from 1922.1 to 2746.2 mAh / g, exhibiting excellent specific capacity.
[0070] Figure 5 These are cycle test graphs of "sandwich" structure lithium metal anodes with lithium strip thicknesses of 20μm (a), 60μm (b), and 100μm (c). Compared to pure lithium strips, the polarization of the "sandwich" structure lithium metal anode during cycling is significantly less than that of batteries assembled from pure lithium sheets, and the cycle life of the modified battery is significantly improved. This indicates that the unique electrode structure and lithiophilic sites reduce ohmic polarization, electrochemical polarization, concentration polarization, and nucleation barrier, suggesting that this structure has great application potential in secondary energy storage batteries.
[0071] Figure 6 These are cycle test graphs for Comparative Example 1 (60μm lithium sheet) and Comparative Example 2. The graphs show that the lithium metal anode with the structure of a carbon fiber film without lithiophilic sites + a 60μm ultrathin lithium strip + an uncarbonized fiber film has a similar cycle life to the lithium metal anode of Example 2. However, the polarization voltage of the lithium metal anode without lithiophilic seed sites at the bottom layer is higher than that with lithiophilic seed sites, indicating that the introduction of lithiophilic sites lowers the lithium nucleation barrier. The lithium metal anode with the structure of a carbon fiber film with lithiophilic sites + a 60μm ultrathin lithium strip has a significantly lower cycle life compared to Example 2, similar to the pure lithium anode, and a significantly higher polarization voltage. This indicates that the "sandwich" structure of the lithium metal anode significantly alleviates the damage caused by lithium dendrites, and the introduction of lithiophilic seed sites lowers the polarization voltage.
[0072] The above embodiments demonstrate that the present invention provides a "sandwich" structure lithium metal anode. The bottom layer is a cross-linked carbonized fibrous membrane with lithium-affinity sites, the middle layer is an ultrathin lithium band, and the top layer is a cross-linked, uncarbonized fibrous membrane. This unique structure guides the directional deposition of lithium in the bottom layer, and the porous structure of the fibrous membrane can accommodate the volume expansion of lithium metal, increasing the transport velocity of lithium ions. The prepared lithium metal anode exhibits excellent energy density and significantly improves the cycle life of lithium metal batteries.
[0073] The above embodiments are merely preferred embodiments of the present invention. Any non-substantial changes and substitutions made by those skilled in the art based on the present invention shall fall within the scope of protection claimed by the present invention.
Claims
1. A metal lithium negative electrode of "sandwich" structure, characterized in that, The lithium metal anode comprises: As the underlying lithium-loving carbon fiber membrane material, The ultra-thin lithium strip as the intermediate layer, and The top layer is an uncarbonized fiber membrane material, wherein the top layer is a porous, non-conductive layer. The lithium-loving carbonized fiber membrane is formed by carbonizing a cross-linked three-dimensional fiber network and then growing nanoscale lithium-loving seed sites on the surface of the fiber filaments. The thickness of the ultrathin lithium strip is less than 100 μm. The uncarbonized fiber membrane material is a cross-linked three-dimensional fiber network that has not undergone carbonization treatment. The thickness of the lithium metal anode is in the range of 80-180 μm.
2. The lithium metal anode of claim 1, wherein, The underlying layer has conductive and lithium-philic properties.
3. The lithium metal anode of claim 1, wherein, The three-dimensional fiber network is formed by electrospinning and cross-linking of polyacrylonitrile and / or polyimide, with the cross-linking of the fibers occurring during the electrospinning film formation process.
4. The lithium metal anode of claim 1, wherein, The lithiophilic seed sites are formed by impregnating the carbonized fiber membrane with a metal salt solution, drying it, and then using microwave heating to provide a heat source to reduce the metal ions.
5. A method of producing a metal lithium negative electrode as defined in any one of claims 1 to 4, characterized in that, The method includes: Electrospinning of polyacrylonitrile and / or polyimide, cross-linking treatment during the formation of fiber membrane, and collection of the spun fiber membrane; The cross-linked fiber membrane is carbonized, and the carbonized fiber membrane is impregnated with a metal salt solution. The impregnated fiber membrane is dried and then microwave-heated to reduce it, thus obtaining a carbonized fiber membrane with lithium affinity. Using the lithium-loving carbonized fiber membrane as the bottom layer, the ultra-thin lithium strip as the middle layer, and the uncarbonized cross-linked fiber membrane as the top layer, the three layers are rolled together using a roller press.
6. The method of claim 5, wherein, The thickness of the ultrathin lithium strip is in the range of 20-100 μm.
7. The method of claim 5, wherein, The cross-linked fiber membrane material that has not undergone carbonization treatment satisfies at least one of the following conditions: The transverse and / or longitudinal breaking strength is 12-40 N; The thickness is 25-60 μm.
8. The method of claim 5, wherein, The crosslinking process involves placing ultraviolet lamps on both sides in front of the electrospinning nozzle and using ultraviolet light to crosslink the fibers.
9. The method of claim 5, wherein, The fiber membrane material impregnated and carbonized with a metal salt solution includes: The fiber membrane material is immersed in a salt solution of silver or gold; The soaked fiber membrane is dried at 40-100℃. Furthermore, the microwave heating reduction includes: Heating at microwave frequencies of 2400-3000 MHz and power of 700-900W for 10-60 s generates in-situ lithium-affinity seed sites on the fiber membrane.
10. The application of the lithium metal anode according to any one of claims 1-4 in a lithium metal battery.
Citation Information
Patent Citations
Nitrogen-doped porous carbon nanofiber composite material for lithium / sodium ion battery negative electrode and preparation method
CN111244412A
Method for preparing conductive fiber paper with lithium-philic and lithium-phobic gradient structure and conductive fiber paper
CN113073496A