High cold upsetting performance and high fatigue performance industrial pure iron large coil

By improving the manufacturing process of large coils of industrial pure iron, the problems of coarse ferrite grains and mixed grains have been solved, improving cold heading performance and fatigue strength, and meeting the special fastener needs of downstream users.

CN117564087BActive Publication Date: 2026-11-24ZENITH STEEL GROUP CORP CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311642761.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2023-10-31
Filing Date
2023-12-04
Publication Date
2026-11-24
Estimated Expiration
2043-12-04

AI Technical Summary

Technical Problem

The production process of industrial pure iron coils involves coarse ferrite grains and mixed crystals, resulting in low cold heading performance and fatigue strength. This makes it impossible to meet the requirements of downstream users for large deformation and high fatigue performance in non-annealed cold heading.

Method used

By employing innovative processes such as converter smelting, LF refining, RH vacuum refining, billet continuous casting, billet grinding, billet heating, roughing and intermediate rolling, pre-finishing rolling, finishing rolling, hot coiling, insulated tunnel cooling, and bundling, we ensure that industrial pure iron coils obtain a uniform, crystal-free microstructure, thereby improving cold heading performance and fatigue performance.

Benefits of technology

It achieves high cold heading performance and high fatigue performance of industrial pure iron large coils, meeting the needs of downstream users for large deformation and high fatigue performance in non-annealed cold heading processing. The 1/6 cold upsetting qualification rate reaches 100%, and the fatigue strength is no less than 5 million cycles with a 50% survival rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention belongs to the field of industrial pure iron technology, specifically relating to a large coil of industrial pure iron with high cold heading and high fatigue performance. The large coil uses continuously cast steel billets produced at high drawing speeds, low superheat, and dynamic reduction as raw material. It is heated in a regenerative furnace, and roughing, intermediate rolling, and pre-finishing are completed using a two-roll mill with alternating horizontal and vertical rolling. Finally, it is finished to the desired specifications using a three-roll mill, then collected using a hot coiler, and finally cooled in a controlled-temperature tunnel. This invention, through process innovation in billet continuous casting and large coil rolling, enables the large coil of industrial pure iron to achieve a uniform, non-mixed-grain microstructure, and effectively improves its cold heading and fatigue performance, meeting the needs of downstream users for non-annealed cold heading of hollow bolts with large deformation and high fatigue performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of industrial pure iron technology, specifically relating to a large coil of industrial pure iron with high cold heading performance and high fatigue performance. Background Technology

[0002] Industrial pure iron is a type of steel whose main chemical component is iron, with a content of 99.50%–99.90%, and a carbon content below 0.04%. The lower the content of other elements, the better. Because it is not actually pure iron, this type of steel, which is close to pure iron, is called industrial pure iron. Generally, industrial pure iron is particularly soft, extremely tough, and has excellent electromagnetic properties. Industrial pure iron has two main uses: one is as a deep-drawing material, which can be stamped into extremely complex shapes; the other is as an electromagnetic material, exhibiting high magnetic induction and low diamagnetic properties. Industrial pure iron is also an important raw material used in the smelting of precision alloys, high-temperature alloys, ultra-low carbon stainless steel, and electrothermal alloys. Currently, domestic industrial pure iron is mainly produced using methods such as electric arc furnaces, oxygen converters, electric arc furnaces with external vacuum decarburization, and oxygen converters with external vacuum decarburization. Industrial pure iron produced by different processes has its own characteristics: 1. Characteristics of pure iron produced by electric arc furnace: This is the earliest method of producing pure iron. The minimum carbon content is 0.025%, and the nitrogen content is relatively high. Due to the carbonization effect of graphite electrodes, it cannot produce pure iron with a lower carbon content. 2. Characteristics of pure iron produced by oxygen converter: It can produce low-carbon pure iron with a carbon content of less than 0.01%, but its oxygen content is high and its nitrogen content is relatively low, so it can only produce industrial pure iron of general quality. 3. Characteristics of high-quality pure iron produced by the combined electric arc furnace or oxygen converter and ladle refining method: The carbon content of the pure iron can be lower than 0.005%, and the content of phosphorus, sulfur, oxygen, nitrogen, and non-metallic inclusions is low. It is currently the highest quality pure iron.

[0003] Industrial pure iron, due to its extremely low carbon content and almost absence of other alloying elements, suffers from coarse ferrite grains and mixed crystals when produced using hot rolling processes. This problem is particularly pronounced when using large coil production lines to produce industrial pure iron with specifications ranging from Φ26.0 to 42.0 mm, making it a significant challenge for the industry. Furthermore, influenced by its chemical composition and metallographic structure, large coils of industrial pure iron exhibit low and unstable cold heading performance and fatigue strength. This makes it impossible for downstream users to meet the requirements of cold heading without annealing, directly cold drawing the hot-rolled large coils to produce special fasteners such as hollow bolts, hollow rivets, and irregularly shaped nuts that require large deformation and high fatigue performance.

[0004] In summary, developing a large coil of industrial pure iron with high cold heading performance and high fatigue performance to meet the needs of downstream users for special fasteners with large deformation and high fatigue performance in non-annealed cold heading processing is an urgent problem that steel mills need to solve. Summary of the Invention

[0005] To address the aforementioned issues, this invention innovates the processes of continuous casting of steel billets and rolling of large coils, enabling industrial pure iron coils with a diameter of Φ26.0~42.0mm to achieve a uniform, non-mixed-crystal microstructure. Simultaneously, it effectively improves the cold heading and fatigue performance of these industrial pure iron coils, meeting the needs of downstream users for non-annealed cold heading of hollow bolts with large deformation and high fatigue performance.

[0006] A high-cold-heading and high-fatigue-resistance industrial pure iron large coil is manufactured through a process flow of converter smelting, LF refining, RH vacuum refining, continuous casting of steel billets, grinding of steel billets, heating of steel billets, roughing and intermediate rolling, pre-finishing rolling, finishing rolling, hot coiling, controlled cooling in an insulated tunnel, and bundling.

[0007] The method for manufacturing large coils of industrial pure iron according to the present invention will be described in detail below.

[0008] Chemical composition: The main chemical composition range of the high cold heading performance and high fatigue performance industrial pure iron coils of the present invention, by weight percentage, is C: ≤0.01%, Si: ≤0.03%, Mn: ≤0.06%, P≤0.015%, S≤0.015%, Al: ≤0.06%, Cr≤0.10%, Ni≤0.10%, Cu≤0.10%, with the remainder being iron and unavoidable impurities.

[0009] Converter smelting: The entire converter smelting process is stirred by bottom blowing argon gas. The tapping temperature is ≥1660℃, and the tapping carbon is controlled within the range of 0.02%~0.05%. At the same time, the tapping P is ≤0.015% and S is ≤0.015%. No deoxidizer or alloy is added during tapping. The tapping slag is lime (600kg / furnace). A double-bar tapping method is adopted to prevent slag from falling.

[0010] LF refining: The LF refining process does not add deoxidizers, but only involves heating. The LF refining end temperature is 1642~1682℃ for the initial casting furnace and 1627~1667℃ for the continuous casting furnace. LF refining uses carbon-free covering agents.

[0011] RH Vacuum Refining: Argon is used as the booster gas in the RH vacuum refining process, with a booster gas flow rate of 80 Nm. 3 / h~100Nm 3 / h, high vacuum time ≥15min, high vacuum degree 800~1200Pa, soft blowing time ≥10min, soft blowing end temperature 1592~1622℃ for open casting furnace, 1577~1607℃ for continuous casting furnace; after circulation ≥8min, take a sample and determine oxygen (without breaking the air), then add 100kg aluminum granules, circulate for 3min and determine oxygen again, then add an appropriate amount of aluminum granules according to the oxygen determination result, adjust the dissolved oxygen content to 10~20ppm, continue circulation ≥5min and then break the air; after RH vacuum refining, the steel ladle should not be filled with carbonized rice husks, only carbon-free covering agent should be added.

[0012] Continuous casting of billets: The continuous casting process of billets adopts high casting speed, low superheat, and dynamic reduction technology: the casting speed is controlled at 3.0±0.2m / min, the secondary cooling water ratio is 1.0L / kg, and special protective slag for ultra-low carbon steel is used; low superheat casting is adopted, with a target liquidus temperature of 1532℃, the superheat of the initial casting furnace is ≤35℃, and the superheat of the continuous casting furnace is ≤20℃; dynamic reduction is adopted, and 4 sets of reduction rollers are used to reduce the liquid phase ratio by a total of 20mm in the range of 40%~90%, and the cross-section of the continuous casting billet after reduction is 140 (±2)mm*168 (±1)mm.

[0013] Steel billet grinding: The steel billet needs to be ground. The grinding method only requires rounding the four corners of the steel billet.

[0014] Billet heating: The billet is heated using a regenerative heating furnace. The preheating section temperature is 750-850℃, the heating section temperature is 850-950℃, and the soaking section temperature is 950-1000℃.

[0015] Roughing, intermediate rolling and pre-finishing rolling: The roughing, intermediate rolling and pre-finishing rolling mills adopt a horizontal and vertical alternating two-roll mill to roll the heated steel billet into intermediate rolled pieces; the number of stands in the roughing and intermediate rolling mill is 14, the number of stands in the pre-finishing rolling mill is 4, and the rolling temperature of the roughing, intermediate rolling and pre-finishing rolling mills is 850-900℃.

[0016] Finishing: The finishing mill uses five three-roll mills to roll the intermediate workpiece to the finished product specifications. The finishing temperature is 700-730℃.

[0017] Hot coiling: The rolled coils are collected and coiled using a hot coiling machine at a temperature of 650–680℃. The applicable specifications for the large coils of this invention are Φ26.0~42.0mm.

[0018] Insulated tunnel cooling: The coiled coils are immediately transferred to the insulated tunnel for controlled cooling. The temperature of the large coils entering the insulated tunnel is controlled at 630-660℃. The large coils enter the insulated tunnel continuously, with all insulation covers of the insulated tunnel fully open, ensuring that the large coils stay in the insulated tunnel for 20-25 minutes at a cooling rate of 0.15-0.16℃ / s. The temperature of the large coils exiting the insulated tunnel is controlled at <450℃. Then, the walking beam fan is turned on to air-cool the temperature of the large coils to <100℃.

[0019] Bundling: After the controlled cooling is completed, the large coils are transferred to the bundling machine for bundling. The bundling temperature is <100℃. A steel strip bundling machine is used, and the bundling pressure is 10-15 tons.

[0020] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0021] This invention innovates the continuous casting and large coil rolling processes of steel billets, resulting in a metallographic structure free of mixed crystals in industrial pure iron large coils. It achieves a 100% pass rate for 1 / 6 cold forging and high plasticity, meeting the downstream users' demand for hollow bolts with large deformation in non-annealed cold heading. Furthermore, this invention requires the produced bolts to possess the following fatigue properties: fatigue strength ≥70MPa under conditions of 50% material survival rate and a fatigue life of not less than 5 million cycles, simultaneously satisfying the downstream users' needs for hollow bolts with large deformation and high fatigue performance in non-annealed cold heading. Attached Figure Description

[0022] Figure 1 Metallographic structure diagram of the industrial pure iron coil produced in Example 1;

[0023] Figure 2 Metallographic structure diagram of the industrial pure iron coil produced in Example 2;

[0024] Figure 3 Metallographic structure diagram of the industrial pure iron coil produced for Comparative Example 1;

[0025] Figure 4 Metallographic structure diagram of the industrial pure iron coil produced in Comparative Example 2;

[0026] Figure 5 Metallographic structure diagram of the industrial pure iron coil produced for Comparative Example 3. Detailed Implementation

[0027] The specific chemical composition of the large coil of industrial pure iron with high cold heading performance and high fatigue performance, as described in this invention, is as follows:

[0028] Wt, %

[0029]

[0030] Large coil manufacturing process: converter smelting—LF refining—RH vacuum refining—continuous casting of billets—grinding of billets—heating of billets—roughing and intermediate rolling—pre-finishing rolling—finishing rolling—hot coiling—insulated tunnel cooling—bundling.

[0031] The applicable specifications for large coils of this invention are Φ26.0~42.0mm, and the embodiment uses Φ32.0mm as an example.

[0032] Example 1

[0033] 1. Chemical composition

[0034] The chemical composition, by weight percentage, is: C: 0.005%, Si: 0.01%, Mn: 0.02%, P: 0.009%, S: 0.004%, Al: 0.02%, Cr: 0.02%, Ni: 0.03%, Cu: 0.01%, with the remainder being iron and unavoidable impurities.

[0035] 2. Steel billet smelting

[0036] Converter smelting: The entire converter smelting process is stirred by bottom blowing argon gas. The tapping temperature is 1665℃, the tapping carbon is 0.03%, the tapping P is 0.010%, and the tapping S is 0.006%. No deoxidizer or alloy is added during tapping. The tapping slag is lime (600kg / furnace). A double-bar tapping method is used to prevent slag from falling.

[0037] LF refining: The LF refining process does not add deoxidizers, but only involves heating. The LF refining end temperature is 1639℃. LF refining uses a carbon-free covering agent.

[0038] RH Vacuum Refining: Argon is used as the booster gas in the RH vacuum refining process, with a booster gas flow rate of 85 Nm. 3 / h, high vacuum time 19min, high vacuum degree 880Pa, soft blowing time 13min, soft blowing end temperature 1588℃; after 12min of circulation, take a sample and determine the oxygen content (without breaking the air), then add 100kg of aluminum granules, circulate for 3min and determine the oxygen content again, then add an appropriate amount of aluminum granules according to the oxygen determination result to adjust the dissolved oxygen content to 14ppm, continue to circulate for 8min and then break the air; after RH vacuum refining, the steel ladle should not be filled with carbonized rice husks, only carbon-free covering agent should be added.

[0039] Continuous casting of billets: The continuous casting process of billets adopts high casting speed, low superheat, and dynamic reduction technology: the casting speed is controlled at 3.0 m / min, the secondary cooling water ratio is 1.0 L / kg, and special protective slag for ultra-low carbon steel is used; low superheat casting is adopted, with a target liquidus temperature of 1532℃, a superheat of 31℃ in the initial casting furnace, and a superheat of 19℃ in the continuous casting furnace; dynamic reduction is adopted, and 4 sets of reduction rollers are used to reduce the liquid phase ratio by a total of 20 mm in the range of 45%~80%, and the cross-section of the continuous casting billet after reduction is 140 (±2) mm * 168 (±1) mm.

[0040] Steel billet grinding: Rounding the four corners of the steel billet.

[0041] 3. Large coil rolling

[0042] Billet heating: The billet is heated using a regenerative heating furnace with a preheating section temperature of 762-840℃, a heating section temperature of 890-935℃, and a soaking section temperature of 955-990℃.

[0043] Roughing, intermediate rolling and pre-finishing rolling: The roughing, intermediate rolling and pre-finishing rolling mills adopt a horizontal and vertical alternating two-roll mill to roll the heated steel billet into intermediate rolled pieces; the number of stands in the roughing and intermediate rolling mill is 14, the number of stands in the pre-finishing rolling mill is 4, and the rolling temperature of the roughing, intermediate rolling and pre-finishing rolling mills is 857 to 880℃.

[0044] Finishing: The finishing mill uses five three-roll mills to roll the intermediate workpiece to the finished product specifications. The finishing temperature is 701-725℃.

[0045] Hot coiling: The rolled coils are collected and coiled using a hot coiling machine at a temperature of 653–670°C.

[0046] Insulated tunnel cooling: The coiled coils are immediately transferred to the insulated tunnel for controlled cooling. The temperature of the large coils entering the insulated tunnel is controlled at 638-648℃. The large coils enter the insulated tunnel continuously, with all insulation covers of the insulated tunnel fully opened, ensuring that the large coils stay in the insulated tunnel for 23 minutes at a cooling rate of 0.15℃ / s. The temperature of the large coils exiting the insulated tunnel is controlled at 431-441℃. Then, the walking beam fan is turned on to air-cool the temperature of the large coils to 85℃.

[0047] Bundling: After the controlled cooling is completed, the large coils are transferred to the bundling machine for bundling. The bundling temperature is 50℃, and a steel strip bundling machine is used with a bundling pressure of 12 tons.

[0048] Example 2

[0049] 1. Chemical composition

[0050] The chemical composition, by weight percentage, is: C: 0.002%, Si: 0.02%, Mn: 0.03%, P: 0.008%, S: 0.008%, Al: 0.03%, Cr: 0.01%, Ni: 0.01%, Cu: 0.02%, with the remainder being iron and unavoidable impurities.

[0051] 2. Steel billet smelting

[0052] Converter smelting: The entire converter smelting process is stirred by bottom blowing argon gas. The tapping temperature is 1670℃, the tapping carbon is 0.02%, the tapping P is 0.008%, and the tapping S is 0.007%. No deoxidizer or alloy is added during tapping. The tapping slag is lime (600kg / furnace). A double-bar tapping method is used to prevent slag from falling.

[0053] LF refining: The LF refining process does not add deoxidizers, but only involves heating. The LF refining end temperature is 1655℃. LF refining uses a carbon-free covering agent.

[0054] RH Vacuum Refining: Argon is used as the booster gas in the RH vacuum refining process, with a booster gas flow rate of 95 Nm. 3 / h, high vacuum time 21min, high vacuum degree 1050Pa, soft blowing time 15min, soft blowing end temperature 1597℃; after 10min of circulation, take a sample and determine the oxygen content (without breaking the air), then add 100kg of aluminum granules, circulate for 3min and determine the oxygen content again, then add an appropriate amount of aluminum granules according to the oxygen determination result to adjust the dissolved oxygen content to 17ppm, continue to circulate for 7min and then break the air; after RH vacuum refining, the steel ladle should not be filled with carbonized rice husks, only carbon-free covering agent should be added.

[0055] Continuous casting of billets: The continuous casting process of billets adopts high casting speed, low superheat, and dynamic reduction technology: the casting speed is controlled at a high speed of 3.2m / min, the secondary cooling water ratio is 1.0L / kg, and special protective slag for ultra-low carbon steel is used; low superheat casting is adopted, with a target liquidus temperature of 1532℃, a superheat of 28℃ in the initial casting furnace, and a superheat of 18℃ in the continuous casting furnace; dynamic reduction is adopted, and 4 sets of reduction rollers are used to reduce the liquid phase ratio by a total of 20mm in the range of 50%~88%, and the cross-section of the continuous casting billet after reduction is 140 (±2)mm*168 (±1)mm.

[0056] Steel billet grinding: Rounding the four corners of the steel billet.

[0057] 3. Large coil rolling

[0058] Billet heating: The billet is heated using a regenerative heating furnace with a preheating section temperature of 766-843℃, a heating section temperature of 888-941℃, and a soaking section temperature of 962-997℃.

[0059] Roughing, intermediate rolling and pre-finishing rolling: The roughing, intermediate rolling and pre-finishing rolling mills adopt a horizontal and vertical alternating two-roll mill to roll the heated steel billet into intermediate rolled pieces; the number of stands in the roughing and intermediate rolling mill is 14, the number of stands in the pre-finishing rolling mill is 4, and the rolling temperature of the roughing, intermediate rolling and pre-finishing rolling mills is 860 to 895℃.

[0060] Finishing: The finishing mill uses five three-roll mills to roll the intermediate workpiece to the finished product specifications. The finishing temperature is 705-728℃.

[0061] Hot coiling: The rolled coils are collected and coiled using a hot coiling machine at a temperature of 651–665°C.

[0062] Insulated tunnel cooling: The coiled coils are immediately transferred to the insulated tunnel for controlled cooling. The temperature of the large coils entering the insulated tunnel is controlled at 628-639℃. The large coils enter the insulated tunnel in a continuous unloading manner. All insulation covers of the insulated tunnel are opened to ensure that the large coils stay in the insulated tunnel for 25 minutes with a cooling rate of 0.16℃ / s. The temperature of the large coils exiting the insulated tunnel is controlled at 388-399℃. Then, the walking beam fan is turned on to air-cool the temperature of the large coils to 70℃.

[0063] Bundling: After the controlled cooling is completed, the large coils are transferred to the bundling machine for bundling. The bundling temperature is 40℃, and a steel strip bundling machine is used with a bundling pressure of 15 tons.

[0064] Comparative Example 1

[0065] In Example 1, step 2 of billet smelting, the continuous casting of billets is replaced with: the continuous casting speed is controlled at 2.0 m / min, the secondary cooling water ratio is 1.0 L / kg, and a special protective slag for ultra-low carbon steel is used; normal superheat casting is adopted, with a target liquidus temperature of 1532℃, a superheat of 50℃ in the initial casting furnace, and a superheat of 40℃ in the continuous casting furnace. Dynamic reduction is not used, and other conditions are the same as in Example 1.

[0066] Comparative Example 2

[0067] Replace the finishing rolling temperature in step 3 of Example 1 with 880-900℃, and keep other conditions the same as in Example 1.

[0068] Comparative Example 3

[0069] In Example 1, step 3 of the large coil rolling process is replaced with the following: the coil is immediately transferred to the insulated tunnel for controlled cooling. The temperature of the large coil entering the insulated tunnel is controlled at 800-900℃. The large coil enters the insulated tunnel continuously, with all insulation covers closed. The large coil remains in the insulated tunnel for 25 minutes at a cooling rate of 0.08℃ / s. The temperature of the large coil exiting the insulated tunnel is controlled at 680-780℃. The walking beam fan is then turned off. Other conditions are the same as in Example 1.

[0070] The industrial pure iron coils / bars produced in the embodiments and comparative examples of this invention are shown in Table 1 below, with the Φ32.0mm specification as an example. The F-grain size, 1 / 6 cold upsetting, and fatigue strength (material under 50% survival rate and fatigue life of not less than 5 million cycles) of the industrial pure iron coils produced using different methods are tested as follows:

[0071] Table 1

[0072]

Claims

1. A large coil of industrial pure iron with high cold heading performance and high fatigue performance, characterized in that: The manufacturing process of industrial pure iron large coils is as follows: converter smelting—LF refining—RH vacuum refining—continuous casting of steel billets—grinding of steel billets—heating of steel billets—roughing and intermediate rolling—pre-finishing rolling—finishing rolling—hot coiling—insulated tunnel cooling—bundling; The chemical composition range of industrial pure iron coils, by weight percentage, is: C: ≤0.01%, Si: ≤0.03%, Mn: ≤0.06%, P: ≤0.015%, S: ≤0.015%, Al: ≤0.06%, Cr: ≤0.10%, Ni: ≤0.10%, Cu: ≤0.10%, with the remainder being iron and unavoidable impurities. The billet continuous casting process employs high casting speed, low superheat, and dynamic reduction technology: the continuous casting speed is controlled at 3.0±0.2m / min, and the secondary cooling water ratio is 1.0L / kg; low superheat casting is used, with a target liquidus temperature of 1532℃, a superheat of ≤35℃ in the initial casting furnace, and a superheat of ≤20℃ in the continuous casting furnace; dynamic reduction is used, with 4 sets of reduction rollers cumulatively reducing the liquid phase by 20mm in the region of 40%~90% liquid phase ratio. Large coil rolling process: billet preheating zone temperature 750~850℃, heating zone temperature 850~950℃, soaking zone temperature 950~1000℃; finishing rolling temperature 700~730℃; the rolled large coil is collected and coiled using a hot coiler at a coiling temperature of 650~680℃; the coiled large coil is immediately transferred to an insulated tunnel for controlled cooling. The temperature of the large coil entering the insulation tunnel is controlled at 630-660℃. The large coil enters the insulation tunnel continuously, with all insulation covers of the insulation tunnel fully open, ensuring that the large coil stays in the insulation tunnel for 20-25 minutes at a cooling rate of 0.15-0.16℃ / s. The temperature of the large coil exiting the insulation tunnel is controlled at <450℃. Subsequently, the walking beam fan is turned on to air-cool the temperature of the large coil to <100℃.

2. The industrial pure iron coil with high cold heading performance and high fatigue performance according to claim 1, characterized in that: The finishing mill uses a 5-stand three-roll mill to roll the intermediate rolled pieces to the finished product specifications; the roughing, intermediate rolling and pre-finishing mills use a horizontal and vertical alternating two-roll mill to roll the heated steel billets into intermediate rolled pieces; the roughing and intermediate rolling mills have 14 stands and the pre-finishing mills have 4 stands, and the rolling temperature of the roughing, intermediate rolling and pre-finishing mills is 850-900℃.

3. The high cold heading performance and high fatigue performance industrial pure iron coil according to claim 2, characterized in that: After the controlled cooling process, the large coils are transferred to a baler for baling. The baling temperature is <100℃. A steel strap baler is used, and the baling pressure is 10-15 tons.

4. The high cold heading performance and high fatigue performance industrial pure iron coil according to claim 3, characterized in that, The industrial pure iron coil has a metallographic structure free of mixed crystals, a 100% pass rate for 1 / 6 cold upsetting, and a fatigue strength ≥70MPa under conditions of 50% survival rate and fatigue life of not less than 5 million cycles. The applicable specifications for the coil are Φ26.0~42.0mm.

Citation Information

Patent Citations

  • Continuous casting method for improving central shrinkage cavity of small high-carbon steel square billet

    CN103506586A

  • Deep-drawing pure iron for high-strength fastening piece and production method of deep-drawing pure iron

    CN105331769A

  • Control method for reducing surface crush damage of wire spring steel

    CN112077140A

  • Industrial pure iron heating and rolling method

    CN114632816A

  • Cold forging steel hot-rolled wire rod for delayed fracture-resistant 14.9-grade quenched and tempered bolt and preparation method of cold forging steel hot-rolled wire rod

    CN116083806A