A method of heat treating a metallized film capacitor
By improving metallized thin-film capacitors through multilayer metal layers and heat treatment methods, the problems of high resistivity, low thermal conductivity and uneven heat treatment are solved, thereby improving the capacitor's current resistance and consistency. It is suitable for high-voltage frequency converters, rail transit, new energy and other fields.
Patent Information
- Application Number
- CN202311225771.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-15
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-01-15
AI Technical Summary
Existing metallized film capacitors suffer from problems such as high resistivity, low thermal conductivity, limitations in welding processes, uneven heat treatment, and short lifespan and insufficient withstand voltage due to moisture residue.
It adopts a multi-layer metal structure, including pure zinc, tin-zinc alloy, pure aluminum and pure copper metal layers, combined with inclined transition layers and edge design, and with hot pressing fixtures and progressive heat treatment methods, to ensure tension release and temperature uniformity of the capacitor core after winding, and uses elastic elements to press to remove air.
It improves the capacitor's current withstand capability, high voltage safety distance, self-healing performance, and current capacity, reduces the failure rate of cold solder joints, and enhances product consistency and energy density. It is suitable for high voltage frequency converters, rail transit, new energy and other fields.
Smart Images

Figure CN117577450B_ABST
Abstract
Description
[0001] Divisional application, original application number: 202210045546.3, application date: January 15, 2022; invention title: A metallized thin film capacitor and its metal layer spraying and heat treatment method. Technical Field
[0002] This invention relates to a capacitor, specifically a heat treatment method for a metallized thin-film capacitor. Background Technology
[0003] Currently, traditional metallized film capacitors are formed by directly spraying pure zinc or zinc-tin alloy onto the winding process to create a single electrode surface, followed by welding. In existing technologies, due to limitations in the welding process, zinc or zinc-tin alloys are mostly used as the capacitor terminal electrode material. However, zinc and zinc-tin alloys have drawbacks such as high resistivity and low thermal conductivity. The resistivity of zinc is 59 nΩ·m and that of tin is 11.4 nΩ·m, while their thermal conductivity is 112 W / mK and 64 W / mK, respectively. When a large current passes through the capacitor terminal electrodes, charge carriers (electrons or holes) are generated and captured by the trap bands of the dielectric and electrodes, forming trapped charges. This leads to structural damage to the material, limiting the capacitor's lifespan and restricting the development of higher current capacities. Furthermore, film capacitors generate a significant amount of heat during use, causing some damage.
[0004] Furthermore, the heat treatment methods used in the production of commonly used metallized film capacitors involve thermally shrinking the polypropylene film in both the radial and transverse directions during processing. This squeezes out the moisture and air remaining within the wound film, improving the tightness between the film layers of the capacitor core. Currently, the conventional heat treatment involves preheating and pressing, followed by heat treatment in an atmospheric or vacuum oven. However, atmospheric oven heat treatment is affected by the heat treatment fixtures and processes, making it difficult to completely squeeze out 100% of the moisture and air remaining within the wound film. Because the air and moisture cannot be completely removed, the current domestic film voltage withstand level cannot be increased to its limit. Air oven heat treatment requires high power, generates significant noise, and operates in a difficult environment. It also heats up slowly, and the large vacuum space prevents uniform temperature distribution, resulting in uneven heating of the product within the oven. This leads to uneven removal of air and moisture between the film layers, resulting in poor consistency in the heat treatment of the capacitor core.
[0005] Therefore, further improvements are necessary. Summary of the Invention
[0006] The purpose of this invention is to provide a heat treatment method for metallized thin-film capacitors to overcome the shortcomings of the prior art.
[0007] A metallized film capacitor designed for this purpose includes a capacitor core, which is a flat core type and is formed by winding at least one polypropylene film. After winding, the upper and lower ends of the capacitor core are respectively coated with several metal layers. The polypropylene film has several vapor-deposited aluminum layers distributed on its surface, and a metal thickening layer is provided on the vapor-deposited aluminum layers, with a margin between adjacent vapor-deposited aluminum layers.
[0008] An inclined transition layer is provided between the thickened metal layer and the vapor-deposited aluminum layer, and the inclined transition layer is inclined downward in the direction of the edge.
[0009] The metal thickening layer is a zinc vapor deposited on the surface of the aluminum vapor deposited layer; the inclined transition layer is a zinc vapor deposited on the surface of the aluminum vapor deposited layer, with one side having the same thickness as the metal thickening layer and the two being connected, and the other side having a thickness that gradually decreases linearly and is connected to the surface of the aluminum vapor deposited layer; among them, the sheet resistance of the inclined transition layer gradually increases as the thickness increases.
[0010] The plurality of metal layers include at least three layers, namely a first layer, a second layer and a third layer; wherein the first layer is the bottom layer and is a pure zinc metal layer or a tin-zinc alloy layer, the second layer is the middle layer and is a pure aluminum metal layer or a pure copper metal layer, and the third layer is the surface layer and is a pure zinc metal layer or a tin-zinc alloy layer.
[0011] A heat treatment method for a metallized film capacitor, comprising the aforementioned metallized film capacitor, wherein the heat treatment method includes the following steps: Step 1: The capacitor core is a flat core type, and after winding, it is placed in a clean winding room with a temperature of 25±5℃ and a humidity of ≤30% for 4-6 hours; Step 2: Place several capacitor cores one by one on each layer of the hot press fixture, then place the hot press fixture on an electric pressure table or a pneumatic pressure table, and apply a pressure of 0.35-0.6MPa to press the capacitor cores together. Then, use fasteners to lock the hot press fixture. Step 3: Place the locked hot press fixture inside the drying equipment, and use the temperature changes of the drying equipment to sequentially heat up, keep warm, heat up again, keep moist, and cool down several capacitor cores. Step 4: Remove the hot press fixture from the drying equipment and disassemble it to complete the heat treatment process of the flat-core capacitor core.
[0012] In step 2, the hot press fixture includes a bracket, on which positioning posts are fixedly mounted. The positioning posts have at least two on the left and right, and each has a threaded portion on its upper part. Several partitions are stacked on the at least two positioning posts from bottom to top. Several capacitor cores are placed one by one between adjacent partitions. A first pressure plate and a second pressure plate are also provided on the uppermost partition. The first pressure plate is located below the second pressure plate, and an elastic element is provided between the two. The elastic element is sleeved on the positioning posts and acts elastically on the first pressure plate and the second pressure plate respectively.
[0013] An electric or pneumatic pressure table applies pressure of 0.35-0.6 MPa to the second pressure plate. The second pressure plate transmits pressure to the first pressure plate through an elastic element. The first pressure plate and several partitions work together to press several capacitor cores together. Then, fasteners are applied to the threaded part to lock the second pressure plate.
[0014] In step 3, the drying equipment is at least an atmospheric drying oven, a tunnel oven, or a forced-air drying oven, and its temperature changes include the following stages: First stage of heating: Raise the room temperature to 85℃ for 30-60 minutes; Second stage of heat preservation: Maintain 85℃ for 2 hours; The third stage of heating: raise the temperature from 85℃ to the highest temperature, and the heating time is 15-30 minutes, where the highest temperature is one of three temperatures: 100℃, 105℃, and 110℃. Fourth stage of heat preservation: Maintain the highest temperature and keep warm for 16-26 hours; The fifth stage of cooling: reducing the maximum temperature to below 50℃ for 4-6 hours.
[0015] The present invention, through the improvement of the above-described structure, has the following advantages compared with the prior art: 1. The edge setting can ensure that there is a certain insulation strength between multiple polypropylene films when the capacitor core is wound, and can also increase the current carrying cross-sectional area of the capacitor core, thereby increasing the current resistance of the capacitor core. At the same time, it can effectively improve the high voltage resistance safety distance of the capacitor core and avoid creepage and arcing.
[0016] 2. Using multiple metal layers as electrodes can improve the voltage withstand strength and self-healing performance of the capacitor core, while also reducing the number of parallel solder joints of the capacitor core and lowering the failure rate of cold solder joints.
[0017] 3. A thickened metal layer is provided on the vapor-deposited aluminum layer, and an inclined transition layer is provided between the two. This not only reduces the loss and ESR of the finished capacitor, but also enhances the current withstand capability and pulse life rating of the finished capacitor. At the same time, it can also reduce the product size and increase the product energy density ratio.
[0018] 4. After winding, the capacitor core is left to stand for 4-6 hours to allow the internal tension to be fully released, ensuring the uniformity of tension between the multiple polypropylene films. Furthermore, the gradual heating and cooling during heat treatment prevents inconsistent shrinkage of the polypropylene films due to rapid temperature changes, ensuring the stability and consistency of shrinkage. Simultaneously, the hot-pressing fixtures used during heat treatment apply increasing pressure to the capacitor cores using elastic elements, compressing them to prevent shrinkage of the capacitor cores during the shaping process. This effectively ensures the complete removal of air from the capacitor cores within the drying equipment, guaranteeing the tightness between the multiple polypropylene films.
[0019] 5. It can be widely applied to products in different industries, such as high-voltage frequency converters, rail transit, and new energy. In particular, it plays a key role in improving the energy efficiency and ensuring the consistency of products in the high-energy-storage pulse capacitor industry. Attached Figure Description
[0020] Figure 1 This is a schematic diagram of the structure of the polypropylene film in a first application example of the present invention.
[0021] Figure 2 This is a schematic diagram of the structure of a second application example of the polypropylene film of the present invention.
[0022] Figure 3 This is a schematic diagram of the structure of the polypropylene film in a third application example of the present invention.
[0023] Figure 4 This is a schematic diagram of a flat-core capacitor core structure.
[0024] Figure 5 This is a schematic diagram of the cross-sectional structure of a flat-core capacitor core.
[0025] Figure 6 for Figure 5 A magnified structural diagram at point B in the diagram.
[0026] Figures 7-9 This is a schematic diagram of the metal layer spraying and placement process for a flat-core capacitor core.
[0027] Figure 10 This is a schematic diagram of a hot-pressing fixture.
[0028] Figure 11 This is a cross-sectional view of the hot pressing fixture.
[0029] Figure 12 This is a schematic diagram of the assembly structure of the electric pressure table and hot press fixture.
[0030] Figure 13 This is a schematic diagram of the pneumatic pressure table and hot press fixture assembly structure.
[0031] Figure 14 , Figure 15 This is a schematic diagram illustrating the process of placing the capacitor core inside an atmospheric drying oven.
[0032] Figure 16 This is a schematic diagram showing the capacitor core placed inside a tunnel furnace. Detailed Implementation
[0033] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0034] See Figures 1-16 The metallized film capacitor includes a capacitor core 1, which is either round or flat and is formed by winding at least one polypropylene film 2. After winding, the upper and lower ends of the capacitor core 1 are coated with several metal layers. The polypropylene film 2 has several vapor-deposited aluminum layers 3 distributed on its surface. A metal thickening layer 4 is provided on the vapor-deposited aluminum layers 3, and an edge 5 is provided between adjacent vapor-deposited aluminum layers 3.
[0035] The setting of the edge 5 can ensure that there is a certain insulation strength between the multiple polypropylene films 2 when the capacitor core 1 is wound, and can also increase the current carrying cross-sectional area of the capacitor core 1, thereby increasing the current resistance of the capacitor core 1. At the same time, it can effectively improve the high voltage resistance safety distance of the capacitor core 1 and avoid creepage and arcing.
[0036] An inclined transition layer 6 is provided between the metal thickening layer 4 and the vapor-deposited aluminum layer 3. The inclined transition layer 6 is inclined downward in the direction of the edge 5.
[0037] The metal thickening layer 4 is a zinc vapor deposited on the surface of the aluminum vapor deposited layer 3; the inclined transition layer 6 is a zinc vapor deposited on the surface of the aluminum vapor deposited layer 3, with one side having the same thickness as the metal thickening layer 4 and the two being connected, and the other side having a thickness that gradually decreases in a straight line and being connected to the surface of the aluminum vapor deposited layer 3; wherein, the sheet resistance of the inclined transition layer 6 gradually increases as the thickness of the inclined transition layer increases.
[0038] like Figure 1 As shown, the capacitor core 1 is made of a polypropylene film 2. Two vapor-deposited aluminum layers 3 are distributed on the surface of the polypropylene film 2. The edge 5 is set between the two vapor-deposited aluminum layers 3 and on the right end of the polypropylene film 2. Meanwhile, a metal thickening layer 4 is provided on the vapor-deposited aluminum layer 3 on the left side. The metal thickening layer 4 has an inclined transition layer 6 on the right side.
[0039] like Figure 2 As shown, the capacitor core 1 is made of two polypropylene films 2 wound together.
[0040] Three vapor-deposited aluminum layers 3 are distributed on the surface of the polypropylene film 2 located at the top. The edge 5 is set between the adjacent vapor-deposited aluminum layers 3. At the same time, the outer ends of the vapor-deposited aluminum layers 3 at both the left and right ends are provided with metal thickening layers 4, and the middle vapor-deposited aluminum layer 3 is provided with metal thickening layers 4 in the middle position.
[0041] Two vapor-deposited aluminum layers 3 are distributed on the surface of the polypropylene film 2 located below. Edges 5 are set between adjacent vapor-deposited aluminum layers 3 and on the polypropylene film 2 at both ends. At the same time, a metal thickening layer 4 is set in the middle of both vapor-deposited aluminum layers 3.
[0042] like Figure 3 As shown, the capacitor core 1 is made of two polypropylene films 2 wound together.
[0043] Three vapor-deposited aluminum layers 3 are distributed on the surface of the polypropylene film 2 located at the top. The edge 5 is set between the adjacent vapor-deposited aluminum layers 3. At the same time, the outer ends of the vapor-deposited aluminum layers 3 at both the left and right ends are provided with metal thickening layers 4. The metal thickening layer 4 at the left end is provided with an inclined transition layer 6 to the right, and the metal thickening layer 4 at the right end is provided with an inclined transition layer 6 to the left. The vapor-deposited aluminum layer 3 in the middle position is provided with a metal thickening layer 4 in the middle position, and the metal thickening layer 4 in the middle position is provided with inclined transition layers 6 to the left and right sides respectively.
[0044] Two vapor-deposited aluminum layers 3 are distributed on the surface of the polypropylene film 2 located below. Edges 5 are set between adjacent vapor-deposited aluminum layers 3 and on the polypropylene film 2 at both ends. At the same time, a metal thickening layer 4 is set in the middle of both vapor-deposited aluminum layers 3, and an inclined transition layer 6 is set on both metal thickening layers 4 to the left and right sides.
[0045] A metal thickening layer 4 is provided on the vapor-deposited aluminum layer 3, and an inclined transition layer 6 is provided between the two. This not only reduces the loss and ESR of the finished capacitor, but also enhances the current withstand capability and pulse life rating of the finished capacitor. At the same time, it can also reduce the product size and increase the product energy density ratio.
[0046] The plurality of metal layers include at least three layers, namely, a first layer 7, a second layer 8, and a third layer 9; wherein, the first layer 7 is the bottom layer and is a pure zinc metal layer or a tin-zinc alloy layer, the second layer 8 is the middle layer and is a pure aluminum metal layer or a pure copper metal layer, and the third layer 9 is the surface layer and is a pure zinc metal layer or a tin-zinc alloy layer.
[0047] Using several metal layers as electrodes can improve the withstand voltage and self-healing performance of capacitor core 1, while also reducing the number of parallel solder joints of capacitor core 1 and lowering the failure rate of cold solder joints.
[0048] A heat treatment method for a metallized film capacitor, comprising the aforementioned metallized film capacitor, wherein the heat treatment method includes the following steps: Step 1: The capacitor core 1 is a flat core type, and after winding, it is placed in a clean winding room with a temperature of 25±5℃ and a humidity of ≤30% for 4-6 hours; Step 2: Place several capacitor cores 1 one by one on each layer of the hot press fixture 13, then place the hot press fixture 13 on the electric pressure table 14 or the pneumatic pressure table 15, and apply a pressure of 0.35-0.6MPa to press the capacitor cores 1 together. Then use fasteners 16 to lock the hot press fixture 13. Step 3: Place the locked hot press clamp 13 into the drying equipment, and use the temperature change of the drying equipment to sequentially heat up, keep warm, heat up again, keep moist, and cool down several capacitor cores 1. Step 4: Remove the hot press fixture 13 from the drying equipment and disassemble the hot press fixture 13 to complete the heat treatment of the flat core capacitor core 1.
[0049] In step 2, the hot press fixture 13 includes a bracket 17, on which a positioning post 18 is fixedly mounted. The positioning post 18 has at least two on the left and right, and each of them has a threaded part on its upper part. Several partitions 19 are stacked on the two positioning posts 18 from bottom to top. Several capacitor cores 1 are placed one by one between adjacent partitions 19. A first pressure plate 20 and a second pressure plate 21 are also provided on the uppermost partition 19. The first pressure plate 20 is located below the second pressure plate 21, and an elastic element 22 is provided between the two. The elastic element 22 is sleeved on the positioning post 18 and acts elastically on the first pressure plate 20 and the second pressure plate 21 respectively.
[0050] The electric pressure table 14 or the pneumatic pressure table 15 applies pressure of 0.35-0.6MPa to the second pressure plate 21. The second pressure plate 21 transmits pressure to the first pressure plate 20 through the elastic element 22. The first pressure plate 20 and several partitions 19 cooperate to press several capacitor cores 1 respectively. Then, the fastener 16 acts on the threaded part and locks the second pressure plate 21.
[0051] Specifically, several flat-core capacitor cores 1 are neatly and centrally placed between adjacent partitions 19. Except for the top and bottom surfaces, the other sides of each flat-core capacitor core 1 should maintain a distance of ≥5mm from the positioning posts 18. Each layer of flat-core capacitor cores 1 is stacked sequentially through the partitions 19, and a first pressure plate 20 is placed when the distance is approximately 50mm. Elastic elements 22 are then fitted onto the left and right positioning posts 18 on the first pressure plate 20. The wire diameter of the elastic elements 22 is ≥1.5mm to ensure the elastic force they generate. Figure 12 As shown, a hot press fixture 13 containing several capacitor cores 1 is placed on an electric pressure table 14, or as shown in the diagram. Figure 13As shown, a hot press jig 13 containing several capacitor cores 1 is placed on a pneumatic pressure table 15. A second pressure plate 21 is then placed on the elastic element 22, and a pressure of 0.4-0.6 MPa is applied to press the capacitor cores 1 together. A gasket 25 and fastener 16 are then placed to lock the second pressure plate 21, ensuring that the pressure F ≥ 150 kg is borne by each layer of flat-core capacitor core 1 in the thickness direction. This process is repeated to obtain a series of hot press jigs 13 containing several capacitor cores 1 for subsequent production.
[0052] The partition 19 is made of galvanized aluminum or 1mm galvanized stainless steel. The first pressure plate 20 and the second pressure plate 21 are made of galvanized and anodized stainless steel. The hot press fixture 13 must be polished during processing to ensure the overall flatness and smoothness of the partition 19, the first pressure plate 20 and the second pressure plate 21, and then galvanized to effectively increase the hardness and smoothness of the hot press fixture 13.
[0053] In step 3, the drying equipment is at least an atmospheric oven 23, a tunnel oven 24, or a forced-air oven, and its temperature changes include the following stages: First stage of heating: Raise the room temperature to 85℃ for 30-60 minutes; Second stage of heat preservation: Maintain 85℃ for 2 hours; The third stage of heating: raise the temperature from 85℃ to the highest temperature, and the heating time is 15-30 minutes, where the highest temperature is one of three temperatures: 100℃, 105℃, and 110℃. Fourth stage of heat preservation: Maintain the highest temperature and keep warm for 16-26 hours; The fifth stage of cooling: reducing the maximum temperature to below 50℃ for 4-6 hours.
[0054] In the third stage of heating and the fourth stage of heat preservation, the setting of the maximum temperature and the length of the heat preservation time are related to the size of capacitor core 1, as can be referred to below: 1. Polypropylene film size: width ≤ 75mm * capacitor core thickness ≤ 25mm * capacitor core width ≤ 135mm, maximum temperature 100℃, and heat preservation time 16-20h.
[0055] 2. Polypropylene film size: width ≤ 75-120mm * capacitor core thickness ≤ 25mm * capacitor core width ≤ 135mm, maximum temperature 105℃, and heat preservation time 20-24h.
[0056] 3. Polypropylene film dimensions: width ≤ 120-150 mm, capacitor core thickness ≤ 25 mm, capacitor core width ≤ 135 mm, maximum temperature 105℃, and heat preservation time 24-26 h.
[0057] like Figure 14 , Figure 15 As shown, a hot press fixture 13 containing several capacitor cores 1 is neatly placed into a transfer cart 26. The bottom of the transfer cart 26 has a directional roller 27, and the bottom of the atmospheric oven 23 has a slot 28. The transfer cart 26 is pushed into the slot 28 of the atmospheric oven 23 by the directional roller 27.
[0058] like Figure 16 As shown, the hot press jig 13, which contains several capacitor cores 1, can be directly and neatly placed into the tunnel furnace 24.
[0059] Compared with existing technologies, the above-described heat treatment method has the following advantages: 1. After the capacitor core 1 is wound, it is left to stand still for 4-6 hours. This ensures that the shrinkage force of the polypropylene film 2 inside the wound capacitor core 1 is not different due to the winding tension. This ensures that the tension inside the wound capacitor core 1 is fully released and that the tension inside the polypropylene film 2 is uniform.
[0060] 2. The heat treatment operation adopts a gradual heating and cooling method to shape and cool down, which avoids the problem of inconsistent film shrinkage caused by rapid temperature changes among multiple polypropylene films 2, and ensures the uniformity of shrinkage among multiple polypropylene films 2.
[0061] 3. The hot press fixture 13 adopts a pressure increment method to ensure that during the shaping process of the capacitor product, the thickness of the capacitor core 1 decreases due to the shrinkage of the polypropylene film 2, and the elastic element 22 expands synchronously. The pressure of the first pressure plate 20 and the second pressure plate 21 on the capacitor core 1 remains unchanged, ensuring that the first pressure plate 20 and the second pressure plate 21 can fully press the capacitor core 1, thereby ensuring that the air inside the capacitor core 1 in the drying equipment is fully removed, and ensuring the tightness between multiple polypropylene films 2.
[0062] 4. The combination of this heat treatment and the hot pressing fixture 13 can effectively ensure that the temperature difference between the inside and outside of the capacitor core 1 is small, and the hot pressing fixture 13 and the capacitor core 1 are in the atmosphere, which can ensure that the capacitor core 1 is heated evenly.
[0063] 5. The adoption of the transfer car 26 can effectively ensure the rapid turnover of capacitor core 1, reduce its turnover time, improve production efficiency, and realize continuous production.
[0064] 6. Effectively ensures the structural stability of the flat-core capacitor core 1. In particular, the withstand voltage of the special large flat-core structure product is greater than or equal to that of the round-core structure. In special application industries, such as high-voltage frequency converters, rail transportation, and new energy, flat-core structure products play a key role in improving energy efficiency and ensuring product consistency, especially in the high-energy-storage pulse capacitor industry. Simultaneously, it provides a solid industrial foundation for the high-density, miniaturization, and lightweighting of metallized film capacitors in applications such as high-energy-storage pulse capacitors, DC support capacitors, and power electronics capacitors. It is particularly suitable for use in microwave oven capacitors.
[0065] The above describes the preferred embodiments of the present invention, illustrating and describing the basic principles, main features, and advantages of the invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as defined by the appended claims and their equivalents.
Claims
1. A heat treatment method for a metallized thin-film capacitor, characterized in that: The metallized film capacitor includes a capacitor core (1), which is a flat core type and is formed by winding at least one polypropylene film (2). After winding, the upper and lower ends of the capacitor core (1) are coated with several metal layers respectively. Among them, several vapor-deposited aluminum layers (3) are distributed on the surface of the polypropylene film (2), and a metal thickening layer (4) is provided on the vapor-deposited aluminum layer (3), and an edge (5) is provided between adjacent vapor-deposited aluminum layers (3). An inclined transition layer (6) is provided between the metal thickening layer (4) and the vapor-deposited aluminum layer (3), and the inclined transition layer (6) is inclined downward in the direction of the edge (5); The metal thickening layer (4) is a zinc vapor deposited on the surface of the aluminum vapor deposited layer (3); the inclined transition layer (6) is a zinc vapor deposited on the surface of the aluminum vapor deposited layer (3), with one side having the same thickness as the metal thickening layer (4) and the two being connected, and the other side having a thickness that gradually decreases in a straight line and being connected to the surface of the aluminum vapor deposited layer (3); wherein, the sheet resistance of the inclined transition layer (6) gradually increases as the thickness of the inclined layer increases; The plurality of metal layers include at least three layers, namely the first layer (7), the second layer (8) and the third layer (9); wherein the first layer (7) is the bottom layer and is a pure zinc metal layer or a tin-zinc alloy layer, the second layer (8) is the middle layer and is a pure aluminum metal layer or a pure copper metal layer, and the third layer (9) is the surface layer and is a pure zinc metal layer or a tin-zinc alloy layer. The heat treatment method includes the following steps: Step 1: The capacitor core (1) is a flat core type, and after winding, it is placed in a clean winding room with a temperature of 25±5℃ and a humidity of ≤30% for 4-6 hours; Step 2: Place several capacitor cores (1) one by one on each layer of the hot press fixture (13), then place the hot press fixture (13) on the electric pressure table (14) or the pneumatic pressure table (15) and apply a pressure of 0.35-0.6MPa to press the capacitor cores (1) together. Then use fasteners (16) to lock the hot press fixture (13). The hot press fixture (13) includes a bracket (17), on which a positioning post (18) is fixedly installed. The positioning post (18) has at least two on the left and right, and the upper part is provided with a threaded part. At least two positioning posts (18) are stacked from bottom to top with several partitions (19). Several capacitor cores (1) are placed one by one between adjacent partitions (19). The uppermost partition (19) is also provided with a first pressure plate (20) and a second pressure plate (21). The first pressure plate (20) is located below the second pressure plate (21), and an elastic element (22) is provided between the two. The elastic element (22) is sleeved on the positioning post (18) and acts elastically on the first pressure plate (20) and the second pressure plate (21) respectively. An electric pressure table (14) or a pneumatic pressure table (15) applies a pressure of 0.35-0.6 MPa to the second pressure plate (21). The second pressure plate (21) transmits pressure to the first pressure plate (20) through an elastic element (22), and presses several capacitor cores (1) together with the cooperation of the first pressure plate (20) and several partitions (19). Then, the fastener (16) acts on the threaded part and locks the second pressure plate (21). Step 3: Place the locked hot press clamp (13) into the drying equipment, and use the temperature change of the drying equipment to sequentially heat up, keep warm, heat up again, keep moist, and cool down several capacitor cores (1); The drying equipment is an atmospheric drying oven (23), a tunnel oven (24), or a forced-air drying oven, and its temperature change includes the following stages: First stage of heating: Raise the room temperature to 85℃ for 30-60 minutes; Second stage of heat preservation: Maintain 85℃ for 2 hours; The third stage of heating: raise the temperature from 85℃ to the highest temperature, and the heating time is 15-30 minutes, where the highest temperature is one of three temperatures: 100℃, 105℃, and 110℃. Fourth stage of heat preservation: Maintain the highest temperature and keep warm for 16-26 hours; Among them, in the third stage of heating and the fourth stage of heat preservation, the setting of the highest temperature and the length of heat preservation time are related to the size of capacitor core 1. Fifth stage of cooling: Reduce the maximum temperature to below 50℃, and the cooling time is 4-6 hours; Step 4: Remove the hot press fixture (13) from the drying equipment and disassemble the hot press fixture (13) to complete the heat treatment of the flat core capacitor core (1).
Citation Information
Patent Citations
Vacuum heat treatment method for thin-film capacitor core
CN113643898A
Multi-inner-string single-side metalized film for pulse capacitor
CN202905468U
Capacitor core hot-pressing shaping clamp
CN213845057U