A GaN layer light emitting diode epitaxial wafer with limited electrons and a preparation method thereof

By introducing a confined electron layer with a specific structure into the GaN epitaxial wafer, the electron overflow problem was solved, improving the luminous efficiency and yield of GaN-based light-emitting diodes, while maintaining hole mobility and achieving higher photoelectric performance.

CN117577752BActive Publication Date: 2026-11-24JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311553211.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-21
Publication Date
2026-11-24
Estimated Expiration
2043-11-21

AI Technical Summary

Technical Problem

In existing GaN-based light-emitting diodes, excessively high electron concentration leads to electron overflow, affecting luminous efficiency and yield. Furthermore, the electron blocking layer simultaneously hinders hole mobility.

Method used

An electron-confining layer is introduced into a GaN epitaxial wafer, comprising a first step layer of alternating BN and InGaN layers, a second step layer of undoped GaN layers, and a third step layer of alternating AlGaN and AlInGaN layers. By controlling the material composition and growth conditions, effective electron confinement and hole channels are formed.

Benefits of technology

It effectively limits electron overflow, improves luminous efficiency and yield, while maintaining hole mobility and enhancing the photoelectric performance of GaN-based light-emitting diodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117577752B_ABST
    Figure CN117577752B_ABST
Patent Text Reader

Abstract

This invention discloses a GaN-based light-emitting diode epitaxial wafer with confined electrons, comprising a substrate, and further comprising a buffer layer, an undoped GaN layer, an N-type GaN layer, an electron-confined layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer sequentially stacked on the substrate. The electron-confined layer comprises a first step layer, a second step layer, and a third step layer stacked sequentially from bottom to top. The first step layer is a periodic structure composed of alternating BN and InGaN layers, the second step layer is an undoped GaN layer, and the third step layer is a periodic structure composed of alternating AlGaN and AlInGaN layers. The light-emitting diode epitaxial wafer of this invention can confine the mobility of a portion of electrons, thereby reducing undesirable photoelectric properties such as electron overflow and improving the luminous efficiency and yield of GaN-based light-emitting diodes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of laser diode technology, and more particularly to a GaN layer light-emitting diode epitaxial wafer with confined electrons and its fabrication method. Background Technology

[0002] Gallium nitride (GaN)-based blue light-emitting diodes (LEDs) are one of the most important inventions of the 20th century and the cornerstone of solid-state lighting. Using blue LEDs to excite yellow phosphors to produce white light, known as fluorescent LED lighting, is the mainstream mode of solid-state lighting today. Its photoelectric conversion efficiency far exceeds that of incandescent and fluorescent lamps, making a significant contribution to global energy conservation and emission reduction.

[0003] The luminous efficiency of a light-emitting diode (LED) is closely related to the radiative recombination efficiency of charge carriers in the quantum well. However, since N-type doping is much easier than P-type doping, the electron concentration in an LED is much higher than that of holes. But too many electrons that do not participate in effective recombination can lead to undesirable photoelectric properties such as electron overflow.

[0004] Currently, the method involves growing an electron blocking layer (AlGaN) after growing a multi-quantum well layer. However, while blocking electrons, it also hinders the mobility of holes. Due to the large effective mass of holes and the low mobility, the hole injection efficiency is low, which affects the luminous efficiency of GaN-based light-emitting diodes. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to provide a GaN layer light-emitting diode epitaxial wafer with confined electrons, which can restrict the mobility of a portion of electrons, thereby reducing adverse photoelectric performance such as electron overflow and improving the luminous efficiency and yield of GaN-based light-emitting diodes.

[0006] To address the aforementioned technical problems, a first aspect of the present invention provides an epitaxial wafer for a GaN-based light-emitting diode with confined electron layers, comprising a substrate, and further comprising, sequentially stacked on the substrate, a buffer layer, an undoped GaN layer, an N-type GaN layer, an electron-confined layer, a multiple quantum well layer, an electron-blocking layer, and a P-type GaN layer, wherein...

[0007] The confined electron layer includes a first step layer, a second step layer, and a third step layer stacked sequentially from bottom to top. The first step layer is a periodic structure composed of alternating BN layers and InGaN layers, the second step layer is an undoped GaN layer, and the third step layer is a periodic structure composed of alternating AlGaN layers and AlInGaN layers.

[0008] As an improvement to the above scheme, in each cycle, the InGaN layer is located above the BN layer, and the AlInGaN layer is located above the AlGaN layer.

[0009] As an improvement to the above scheme, the number of cycles of the first step layer is 5 to 10;

[0010] The number of cycles in the third step is 3 to 5.

[0011] As an improvement to the above scheme, the thickness of the BN layer is 5-10 nm, and the thickness of the InGaN layer is 5-10 nm;

[0012] The thickness of the AlGaN layer is 10–20 nm, and the thickness of the AlInGaN layer is 10–20 nm.

[0013] As an improvement to the above scheme, the thickness of the second step layer is 150–200 nm.

[0014] As an improvement to the above scheme, the In composition in the InGaN layer is 0.01 to 0.1, and the In composition shows a decreasing trend with the increase of the period;

[0015] The Al content in the AlGaN layer is 0.05–0.07.

[0016] The Al content in the AlInGaN layer is 0.05 to 0.1, and the Al content increases with the increase of the period; the In content is 0.01 to 0.05.

[0017] As an improvement to the above scheme, the carrier gas used in the growth of the first step layer is N2 (nitrogen);

[0018] The carrier gases used in the growth of the second and third steps are N2 and H2 (hydrogen), with a flow rate ratio of N2 to H2 of 5:1 to 10:1.

[0019] As an improvement to the above scheme, the growth temperature of the first step layer is 800-850℃;

[0020] The growth temperature of the second step layer is 900–1000℃;

[0021] The growth temperature of the third step layer is 900–1000℃.

[0022] As an improvement to the above scheme, the growth pressure of the confined electron layer is 100 to 300 torr.

[0023] A second aspect of the present invention also provides a method for fabricating a GaN layer light-emitting diode epitaxial wafer with confined electrons, characterized in that it includes:

[0024] S1. Provide the substrate described above;

[0025] S2. A buffer layer is grown on the substrate;

[0026] S3. An undoped GaN layer, an N-type GaN layer, an electron-confined layer, a multiple quantum well layer, an electron-blocking layer, and a P-type GaN layer are sequentially grown on the buffer layer.

[0027] The confined electron layer comprises a first step layer, a second step layer, and a third step layer stacked sequentially from bottom to top. The first step layer is a periodic structure composed of alternating BN and InGaN layers, the second step layer is an undoped GaN layer, and the third step layer is a periodic structure composed of alternating AlGaN and AlInGaN layers.

[0028] Implementing this invention has the following beneficial effects:

[0029] The epitaxial wafer of this invention also includes a confined electron layer disposed between the N-type GaN layer and the multiple quantum well layer. Specifically, it includes a first-step layer composed of alternating stacked BN and InGaN layers, and a third-step layer composed of undoped GaN layers and alternating stacked AlGaN and AlInGaN layers. The confined electron layer has high crystal quality and has a certain ability to bind electrons in the main channel of carrier transport. It does not hinder the mobility of holes and has a certain gain effect on the output current, thereby reducing adverse photoelectric performance such as electron overflow and improving the luminous efficiency and yield of GaN-based light-emitting diodes. Attached Figure Description

[0030] Figure 1 : A schematic diagram of the structure of an ultraviolet light-emitting diode epitaxial wafer provided in Embodiment 1 of the present invention;

[0031] Figure 2 : A schematic diagram of the confined electron layer provided in Embodiment 1 of the present invention. Attached image description:

[0033] 100 - Substrate; 200 - Buffer layer; 300 - Undoped GaN layer; 400 - N-type GaN layer; 500 - Confined electron layer; 510 - First step layer; 511 - BN layer; 512 - InGaN layer; 520 - Second step layer; 530 - Third step layer; 531 - AlGaN layer; 532 - AlInGaN layer; 600 - Multiple quantum well layer; 700 - Electron blocking layer; 800 - P-type GaN layer. Detailed Implementation

[0034] To make the objectives, technical solutions, and advantages of the present invention clearer, specific embodiments will be described in further detail below.

[0035] Please see Figure 1 This invention provides an electron-confined GaN layer light-emitting diode epitaxial wafer, comprising a substrate 100, and further comprising a buffer layer 200, an undoped GaN layer 300, an N-type GaN layer 400, an electron-confined layer 500, a multiple quantum well layer 600, an electron blocking layer 700, and a P-type GaN layer 800 sequentially stacked on the substrate 100, wherein...

[0036] The confined electron layer 500 includes a first step layer 510, a second step layer 520, and a third step layer 530 stacked sequentially from bottom to top. The first step layer 510 is a periodic structure composed of alternating BN layers 511 and InGaN layers 512. The second step layer 520 is an undoped GaN layer. The third step layer 530 is a periodic structure composed of alternating AlGaN layers 531 and AlInGaN layers 532.

[0037] In the first stage, the layer thickness is relatively thin, and the surface is under tensile stress and in a strain state. The piezoelectric polarization field in the InGaN layer 512 is directed downwards, and polarized positive charges accumulate on the lower surface of the InGaN layer 512. Correspondingly, a high concentration of electrons appears on the other side of the InGaN layer 512 surface. Since AlGaN, GaN, and InGaN have the same symmetry, the difference in lattice constants causes all strained layers to be subjected to surface tensile stress. The direction of the internal polarization field is generally consistent, but AlGaN is subjected to stronger surface tensile stress, resulting in an increase in polarized positive charges on the lower surface. In the third stage, the conduction band at the interface of the AlGaN layer 531 and the AlInGaN layer 532 heterojunction is lower, which deepens the potential barrier depth at the interface of the AlGaN layer 531 and the AlInGaN layer 532, exhibiting localization of electrons.

[0038] Furthermore, the first step layer 510 has 5 to 10 cycles, with the InGaN layer 512 located above the BN layer 511 in each cycle. The thickness of the BN layer 511 is 5 to 10 nm, exemplarily 5 nm, 5.5 nm, 6 nm, 6.5 nm, 7 nm, 7.5 nm, 8 nm, 8.5 nm, 9 nm, 9.5 nm, and 10 nm, but not limited thereto. The thickness of the InGaN layer 512 is 5 to 10 nm, exemplarily 5 nm, 5.5 nm, 6 nm, 6.5 nm, 7 nm, 7.5 nm, 8 nm, 8.5 nm, 9 nm, 9.5 nm, and 10 nm, but not limited thereto.

[0039] The third-step layer 530 has 3 to 5 cycles. In each cycle, the AlInGaN layer 532 is located above the AlGaN layer 531. The thickness of the AlGaN layer 531 is 10 to 20 nm, exemplarily 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, and 20 nm, but not limited to these. The thickness of the AlInGaN layer 532 is 10 to 20 nm, exemplarily 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, and 20 nm, but not limited to these.

[0040] Furthermore, the In composition in the InGaN layer 512 is 0.01 to 0.1%, and the In composition decreases with increasing period, for example, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, and 0.1, but not limited to these. The larger the In composition in the first-stage layer, the more InGaN gradually becomes the main channel for carrier transport, with a stronger ability to bind electrons within the channel, thus having a certain gain effect on the output current.

[0041] The Al composition in AlInGaN layer 532 is 0.05–0.1%, and the Al composition increases with increasing period, exemplarily 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, but not limited to these. The In composition is 0.01–0.05%, exemplarily 0.01, 0.02, 0.03, 0.04, 0.05, but not limited to these. The Al composition in AlGaN layer 531 remains constant at 0.05–0.07, preferably 0.06. The increasing Al composition in AlInGaN layer 532 with increasing period, while the constant Al composition in AlGaN layer 531, results in a deeper barrier depth at the interface between AlGaN layer 531 and AlInGaN layer 532, enhancing the localization of electrons.

[0042] In this invention, the thickness of the second step layer 520 is 150-200nm, and exemplary thicknesses are 150nm, 155nm, 160nm, 165nm, 170nm, 175nm, 180nm, 185nm, 190nm, 195nm, and 200nm, but it is not limited thereto.

[0043] In this invention, the first-stage layer growth atmosphere is N2 to reduce side reactions and thus avoid a decrease in B / In doping efficiency. The second and third-stage layer growth atmospheres are N2 and H2. Introducing H2 can improve the crystal quality of the confined electron layer 500 and increase atomic mobility, thereby increasing the yield of the light-emitting diode. The N2 to H2 flow ratio is 5:1 to 10:1, with exemplary values ​​of 5:1, 6:1, 7:1, 8:1, 9:1, and 10:1, but not limited to these.

[0044] Accordingly, the present invention also provides a method for fabricating a GaN layer light-emitting diode epitaxial wafer with confined electrons, comprising:

[0045] S1. Provide a substrate 100;

[0046] The substrate 100 of this invention can be selected from one of the following: sapphire substrate, SiO2-sapphire composite substrate, silicon substrate, silicon carbide substrate, gallium nitride substrate, and zinc oxide substrate; more preferably, it is a sapphire substrate. Sapphire, as a GaN-based LED substrate material, has advantages such as mature technology, good stability, and low production cost.

[0047] S2. Grow a buffer layer 200 on the substrate 100;

[0048] In this invention, the buffer layer 200 is an AlN buffer layer. The thickness of the buffer layer 200 is 10–50 nm, more preferably 10–20 nm. Using an AlN buffer layer can control crystal defects, improve the quality of subsequent crystal growth, and alleviate the stress caused by lattice mismatch and thermal mismatch between the substrate 100 and the epitaxial layer.

[0049] Furthermore, the carrier gas can be one of the following: high-purity H2, high-purity N2, or a mixture of high-purity H2 and high-purity N2.

[0050] S3. On the buffer layer 200, sequentially grow an undoped GaN layer 300, an N-type GaN layer 400, an electron-confining layer 500, a multiple quantum well layer 600, an electron-blocking layer 700, and a P-type GaN layer 800.

[0051] In this invention, when growing an undoped GaN layer 300 on the buffer layer 200, the substrate 100 on which the buffer layer 200 has been deposited needs to be pretreated. Specifically, the substrate 100 on which the buffer layer 200 has been deposited is first pretreated in an H2 atmosphere at a temperature of 1000–1200°C for 1–10 min, followed by nitriding. This pretreatment can improve the crystal quality of the buffer layer 200 and effectively improve the crystal quality of the subsequently deposited GaN epitaxial layer.

[0052] Furthermore, the growth temperature of the undoped GaN layer 300 is 1050℃~1200℃, and the growth pressure is 100~600 torr. The higher growth temperature and lower pressure of the undoped GaN layer 300 result in superior GaN crystal quality. The thickness of the undoped GaN layer 300 is 1~5μm. As the thickness of the undoped GaN layer 300 increases, compressive stress is released through stacking faults, line defects are reduced, crystal quality is improved, and reverse leakage current is reduced. However, increasing the thickness of the undoped GaN layer 300 consumes a significant amount of Ga source material, greatly increasing the epitaxial cost of the LED. Therefore, the preferred thickness of the undoped GaN layer 300 is 2~3μm, which not only saves production costs but also ensures high crystal quality of the GaN material.

[0053] In this invention, the N-type GaN layer 400 is a Si-doped GaN layer with a Si doping concentration of 1×10⁻⁶. 19 ~5×10 19 atoms / cm 3 The N-type GaN layer 400 provides sufficient electrons for LED light emission, and its resistivity is higher than that of the transparent electrode on the P-type GaN layer 800. Therefore, sufficient Si doping can effectively reduce the resistivity of the N-type GaN layer 400. The thickness of the N-type GaN layer 400 is 2–3 μm; sufficient thickness can effectively relieve stress and improve the luminous efficiency of the LED.

[0054] Furthermore, the growth temperature of the N-type GaN layer 400 is 1050–1200℃, and the growth pressure is 100–600 torr.

[0055] The multi-quantum well layer 600 in this invention is a composite layer of alternately stacked InGaN quantum well layers and AlGaN quantum barrier layers, with a stacking period of 6 to 12. The InGaN quantum well layers have an In composition of 0.1 to 0.3 and a thickness of 2 to 5 nm; the AlGaN quantum barrier layers have an Al composition of 0.01 to 0.1 and a thickness of 5 to 15 nm. The multi-quantum well layer 600 is a region where electrons and holes recombine. The multi-quantum well layer 600 formed by the alternating stacking of InGaN and AlGaN quantum barrier layers can significantly increase the overlap of electron and hole wave functions, thereby improving the luminous efficiency of LED devices.

[0056] Furthermore, the growth temperature of the InGaN quantum well layer is 790–810 °C, and the growth pressure is 50–300 torr; the growth temperature of the AlGaN quantum barrier layer is 800–900 °C, and the growth pressure is 50–300 torr.

[0057] The electron blocking layer 700 in this invention is an AlGaN layer with an Al composition of 0.005 to 0.1 and a thickness of 10 to 40 nm.

[0058] Furthermore, the electron blocking layer 700 is grown at a temperature of 900–1000°C and a growth pressure of 100–300 torr.

[0059] The p-type GaN layer 800 in this invention is a Mg-doped GaN layer with a Mg doping concentration of 1×10⁻⁶. 19 ~1×10 21 atoms / cm 3 The thickness is 10–50 nm.

[0060] Furthermore, the growth temperature of the P-type GaN layer 800 is 900–1050 °C, and the growth pressure is 100–600 torr.

[0061] It should be noted that in this invention, high-purity NH3 is used as the N source, diborane (B2H6) as the B source, trimethylgallium (TMGa) or triethylgallium (TEGa) as the gallium source, trimethylindium (TMIn) as the indium source, trimethylaluminum (TMAl) as the aluminum source, silane (SiH4) as the N-type dopant, and magnesium pyrocene (CP2Mg) as the P-type dopant for epitaxial growth.

[0062] The present invention will be further described below with reference to specific embodiments:

[0063] Example 1

[0064] This embodiment provides an electron-restricted GaN layer light-emitting diode epitaxial wafer, which, from bottom to top, includes: a substrate 100, a buffer layer 200, an undoped GaN layer 300, an N-type GaN layer 400, an electron-restricted layer 500, a multiple quantum well layer 600, an electron blocking layer 700, and a P-type GaN layer 800. The electron-restricted layer 500 includes a first step layer 510, a second step layer 520, and a third step layer 530 stacked from bottom to top.

[0065] It is obtained by the following preparation method:

[0066] (1) Deposit an AlN buffer layer 200 on substrate 100.

[0067] An AlN buffer layer 200 with a thickness of 15 nm was deposited on a sapphire substrate 100 using a Midea A7 MOCVD (Metal-organic Chemical Vapor Deposition) system with high-purity H2 as the carrier gas.

[0068] (2) Pretreatment of the substrate 100 with the deposited buffer layer 200

[0069] The sapphire substrate 100 with the AlN buffer layer 200 deposited was transferred into MOCVD and pretreated in H2 atmosphere for 5 min at a processing temperature of 1100℃, and then the sapphire substrate 100 was subjected to nitriding treatment.

[0070] (3) Deposit an undoped GaN layer 300 on the AlN buffer layer 200.

[0071] The growth temperature was 1100℃, the growth pressure was 150 torr, and the growth thickness was 2-3 μm.

[0072] (4) Deposit an N-type GaN layer 400 on the undoped GaN layer 300.

[0073] The Si doping concentration is 2.5 × 10⁻⁶. 19 atoms / cm 3 The growth temperature was 1120℃, the growth pressure was 100 torr, and the growth thickness was 2-3 μm.

[0074] (5) Deposit an electron-confining layer 500 on the N-type GaN layer 400.

[0075] The confined electron layer 500 includes a first step layer 510, a second step layer 520, and a third step layer 530 stacked sequentially from bottom to top. The first step layer 510 is a periodic structure composed of alternating BN layers 511 and InGaN layers 512, with a period number of 7. In each period, the InGaN layer 512 is located above the BN layer 511. The In content in the InGaN layer 512 decreases from 0.1 to 0.01 with each period. The growth temperature is 825℃, the pressure is 200 torr, and the carrier gas is N2. The thickness of the BN layer 511 is 7nm, the thickness of the InGaN layer 512 is 8nm, and the total thickness is 105nm.

[0076] The second step layer 520 is an undoped GaN layer with a thickness of 175 nm; the growth temperature is 950 °C, the pressure is 200 torr, and the carrier gas is N2.

[0077] The third-step layer 530 is a periodic structure composed of alternating AlGaN layers 531 and AlInGaN layers 532, with 4 cycles. In each cycle, the AlInGaN layer 532 is located above the AlGaN layer 531. The Al content in the AlGaN layer 531 is 0.06, and the Al content in the AlInGaN layer 532 increases from 0.05 to 0.1 with the increase of the cycle, while the In content is 0.03. The growth temperature is 950℃, the growth pressure is 200 torr, and the carrier gas is N2. The thickness of the AlGaN layer 531 is 15 nm, the thickness of the AlInGaN layer 532 is 15 nm, and the total thickness is 120 nm.

[0078] (6) Deposit a multi-quantum-well layer 600 on the confined electron layer 500.

[0079] The multi-quantum-well layer 600 consists of alternating stacked InGaN quantum well layers and AlGaN quantum barrier layers, with a stacking period of 10. The InGaN quantum well layer has an In composition of 0.22, a growth temperature of 795℃, and a growth pressure of 200 torr. The AlGaN quantum barrier layer has an Al composition of 0.05, a growth temperature of 855℃, and a growth pressure of 200 torr. The InGaN quantum well layer has a thickness of 3.5 nm, the AlGaN quantum barrier layer has a thickness of 9.8 nm, and the total thickness is 133 nm.

[0080] (7) Deposit an electron blocking layer 700 on the multi-quantum well layer 600.

[0081] The electron blocking layer 700 is an AlGaN layer, in which the Al composition concentration gradually increases from 0.01 to 0.05 along the growth direction of the epitaxial layer, the growth temperature is 965℃, the growth pressure is 200 torr, and the thickness is 15nm.

[0082] (8) Deposit a P-type GaN layer 800 on the electron blocking layer 700.

[0083] In the p-type GaN layer 800, the Mg doping concentration is 2×10⁻⁶. 20 atoms / cm 3 The growth temperature was 985℃, the growth pressure was 200 torr, and the thickness was 15nm.

[0084] Example 2

[0085] This embodiment provides a GaN layer light-emitting diode epitaxial wafer with confined electrons, which is basically the same as that in Embodiment 1, except that:

[0086] In the confined electron layer 500, the first step layer 510 has 5 cycles and a total thickness of 75 nm; the second step layer 520 has a thickness of 150 nm; and the third step layer 530 has 3 cycles and a total thickness of 90 nm.

[0087] Example 3

[0088] This embodiment provides a GaN layer light-emitting diode epitaxial wafer with confined electrons, which is basically the same as that in Embodiment 1, except that:

[0089] In the confined electron layer 500, the first step layer 510 has 10 cycles and a total thickness of 150 nm; the second step layer 520 has a thickness of 200 nm; and the third step layer 530 has 5 cycles and a total thickness of 150 nm.

[0090] Example 4

[0091] This embodiment provides a GaN layer light-emitting diode epitaxial wafer with confined electrons, which is basically the same as that in Embodiment 1, except that:

[0092] In the confined electron layer 500, the carrier gas of the first step layer 510 is N2; the carrier gas of the second step layer 520 is N2 and H2 with a flow ratio of 8:1; and the carrier gas of the third step layer 530 is N2 and H2 with a flow ratio of 5:1.

[0093] Comparative Example 1

[0094] This comparative example provides a GaN layer light-emitting diode epitaxial wafer, which is basically the same as that in Example 1, except that:

[0095] It does not contain the restricted electron layer 500.

[0096] Comparative Example 2

[0097] This comparative example provides a GaN layer light-emitting diode epitaxial wafer, which is basically the same as that in Example 1, except that:

[0098] The confinement electron layer 500 includes a first step layer 510 and a second step layer 520 stacked sequentially from bottom to top, but does not include a third step layer 530.

[0099] Comparative Example 3

[0100] This comparative example provides a GaN layer light-emitting diode epitaxial wafer, which is basically the same as that in Example 1, except that:

[0101] The confined electron layer 500 includes a second step layer 520 and a third step layer 530 stacked sequentially from bottom to top, but does not include the first step layer 510.

[0102] Performance testing:

[0103] The epitaxial wafers obtained in Examples 1-4 and Comparative Examples 1-3 were fabricated into 10mil*24mil chips using the same chip process conditions. 300 LED chips were randomly selected from each chip and tested at 120mA / 60mA current. The test results are shown in the table below. The improvement in luminous efficiency and yield was calculated based on Comparative Example 1.

[0104] Table 1. Test results of Examples 1-4 and Comparative Examples 1-3

[0105] Luminous efficiency improvement / % Yield / % XRD 002 / 102 Example 1 2.1 4.8 116 / 136 Example 2 1.9 3.6 134 / 149 Example 3 2.5 4.3 125 / 143 Example 4 3.8 5.3 100 / 130 Comparative Example 1 0 0 180 / 195 Comparative Example 2 1.2 0.9 136 / 167 Comparative Example 3 0.9 1.3 129 / 153

[0106] The experimental data above show that implementing the technical solution of this invention can improve the luminous efficiency by 1% to 4%, increase the yield by 3% to 6%, and maintain good electrical performance in other aspects. Compared with Comparative Example 1, the present invention provides a confined electron layer 500 with a specific structure between the N-type GaN layer 400 and the multi-quantum well layer 600, resulting in a significant improvement in both the luminous efficiency and yield of the obtained light-emitting diode. Compared with Comparative Examples 2 and 3, it can be shown that the first, second, and third step layers in the confined electron layer have a synergistic effect, exhibiting localization of electrons without hindering hole mobility, and providing a certain gain effect on the output current, thereby reducing adverse photoelectric performance such as electron overflow and significantly improving the luminous efficiency and yield of GaN-based light-emitting diodes. Furthermore, Examples 1 and 4 demonstrate that introducing H2 into the atmosphere of the second and third stage layers can improve the crystal quality of the confined electron layer and increase atomic mobility, thereby increasing the yield of the light-emitting diode.

[0107] The above description is merely a preferred embodiment of the present invention and should not be construed as limiting the scope of the invention. Therefore, any equivalent variations made in accordance with the claims of the present invention are still within the scope of the present invention.

Claims

1. A GaN layer light-emitting diode epitaxial wafer with confined electrons, comprising a substrate, characterized in that, It also includes a buffer layer, an undoped GaN layer, an N-type GaN layer, an electron-confining layer, a multiple quantum well layer, an electron-blocking layer, and a P-type GaN layer sequentially stacked on the substrate, wherein, The confined electron layer includes a first step layer, a second step layer and a third step layer stacked sequentially from bottom to top. The first step layer is a periodic structure composed of alternating stacked BN layers and InGaN layers, the second step layer is an undoped GaN layer, and the third step layer is a periodic structure composed of alternating stacked AlGaN layers and AlInGaN layers. In each cycle, the InGaN layer is located above the BN layer, and the AlInGaN layer is located above the AlGaN layer; The thickness of the BN layer is 5~10nm, and the thickness of the InGaN layer is 5~10nm; The thickness of the AlGaN layer is 10~20nm, and the thickness of the AlInGaN layer is 10~20nm.

2. The GaN layer light-emitting diode epitaxial wafer with confined electrons as described in claim 1, characterized in that, The number of cycles in the first step layer is 5 to 10; The number of cycles in the third step is 3 to 5.

3. The GaN layer light-emitting diode epitaxial wafer with confined electrons as described in claim 1, characterized in that, The total thickness of the second step layer is 150~200nm.

4. The GaN layer light-emitting diode epitaxial wafer with confined electrons as described in claim 1, characterized in that, The InGaN layer has an In content of 0.01 to 0.1, and the In content decreases with increasing period. The Al content in the AlGaN layer is 0.05~0.07; The Al content in the AlInGaN layer is 0.05~0.1, and the Al content shows an increasing trend with the increase of the period. The In component is 0.01~0.

05.

5. The GaN layer light-emitting diode epitaxial wafer with confined electrons as described in claim 1, characterized in that, The carrier gas used in the growth of the first step layer is N2; The carrier gases used in the growth of the second and third steps are N2 and H2, with a flow rate ratio of N2 to H2 of 5:1 to 10:

1.

6. The GaN layer light-emitting diode epitaxial wafer with confined electrons as described in claim 1, characterized in that, The growth temperature of the first step layer is 800~850℃; The growth temperature of the second step layer is 900~1000℃; The growth temperature of the third step layer is 900~1000℃.

7. The GaN layer light-emitting diode epitaxial wafer with confined electrons as described in claim 1, characterized in that, The growth pressure of the confined electron layer is 100~300 torr.

8. A method for fabricating a GaN layer light-emitting diode epitaxial wafer with confined electrons as described in any one of claims 1 to 7, characterized in that, include: S1. Provide the substrate described above; S2. A buffer layer is grown on the substrate; S3. An undoped GaN layer, an N-type GaN layer, an electron-confined layer, a multiple quantum well layer, an electron-blocking layer, and a P-type GaN layer are sequentially grown on the buffer layer. The confined electron layer comprises a first step layer, a second step layer, and a third step layer stacked sequentially from bottom to top. The first step layer is a periodic structure composed of alternating BN and InGaN layers, the second step layer is an undoped GaN layer, and the third step layer is a periodic structure composed of alternating AlGaN and AlInGaN layers.

Citation Information

Patent Citations

  • Epitaxial growth method for effectively improving reverse electric leakage of gallium nitride based light-emitting diode

    CN103811605A

  • Light emitting element and light emitting element manufacturing method

    JP2016129180A