High-performance lithium manganese iron phosphate positive electrode material, preparation method thereof and lithium ion battery

By coating lithium manganese iron phosphate composite material with carbon doped with MXene, a three-dimensional porous hierarchical structure is formed, which solves the problems of conductivity and lithium-ion diffusion in lithium manganese iron phosphate cathode material and improves the overall performance of lithium-ion batteries.

CN117577813BActive Publication Date: 2026-11-24HEFEI GUOXUAN HIGH TECH POWER ENERGY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311740569.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-18
Publication Date
2026-11-24
Estimated Expiration
2043-12-18

AI Technical Summary

Technical Problem

The increased manganese content in lithium iron phosphate cathode materials leads to manganese precipitation, which disrupts the solid solution structure, resulting in low electronic conductivity and ion mobility, thus affecting their commercial applications.

Method used

A carbon-coated lithium manganese iron phosphate composite material using MXene doped with polyethylene terephthalate as the carbon source was employed. During high-temperature calcination, lithium manganese iron phosphate was coated and formed into a three-dimensional porous hierarchical conductive network structure, thereby improving the material's conductivity and lithium-ion diffusion capability.

Benefits of technology

It significantly improves the conductivity and rate performance of the material, while also improving low-temperature performance, thus enhancing the capacitance and overall performance of the lithium-ion battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004612940770000081
    Figure BDA0004612940770000081
  • Figure HDA0004612940780000011
    Figure HDA0004612940780000011
Patent Text Reader

Abstract

This invention discloses a high-performance lithium manganese iron phosphate cathode material, its preparation method, and a lithium-ion battery. The preparation method of the lithium manganese iron phosphate cathode material of this invention includes the following steps: S1, activating a single-layer or few-layer MXene two-dimensional material to remove residual surface groups, obtaining MXene nanosheets; S2, reacting a system of dimethyl benzoate, ethylene glycol, and a lithium manganese iron phosphate precursor to generate polyethylene terephthalate and coat the lithium manganese iron phosphate precursor; S3, uniformly mixing the MXene nanosheets obtained in step S1 and the polyethylene terephthalate-coated lithium manganese iron phosphate precursor obtained in step S2, followed by heat treatment to obtain the lithium manganese iron phosphate cathode material. The cathode material of this invention has a three-dimensional porous hierarchical conductive network structure, which significantly improves the material's conductivity and provides channels for lithium-ion diffusion, ensuring sufficient contact with the electrolyte and improving the material's rate capability and low-temperature performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery material technology, and particularly relates to a high-performance lithium manganese iron phosphate cathode material, its preparation method, and a lithium-ion battery. Background Technology

[0002] In recent years, the new energy vehicle industry has flourished, and power batteries such as lithium-ion batteries have gained a vast market. Cathode materials, as a core component of lithium-ion batteries, have always been a top priority in research and development. With increasingly stringent safety requirements, lithium iron phosphate (LFP) cathode materials have become favored by manufacturers due to their high safety and low cost. As an upgrade to LFP, doping with a certain proportion of manganese retains the stable olivine-type structure of LFP while increasing energy density by raising the voltage, thus addressing its energy density shortcomings. Lithium manganese iron phosphate (LMP) combines the advantages of both LFP and ternary materials, maintaining low cost and high safety while also achieving long cycle life and high energy density, making it a popular development direction.

[0003] MXene is a two-dimensional material that provides more channels for ion movement and exhibits superior properties in terms of oxidation resistance and chemical stability, making it widely used in chemical energy storage. Polyethylene terephthalate (PET), with the chemical formula (C... 10 H8O4) n It is prepared by first synthesizing dihydroxyethyl terephthalate by transesterification of dimethyl terephthalate and ethylene glycol or by esterification of terephthalic acid and ethylene glycol, and then carrying out a polycondensation reaction.

[0004] Lithium manganese iron phosphate (LFP) materials have many advantages, but the increased manganese content leads to manganese precipitation, which in turn damages the solid solution structure. At the same time, it reduces the proportion of iron content, resulting in a decrease in rate capability and discharge efficiency. Compared with the 0.3 eV transition band gap of lithium iron phosphate, the transition band gap of electrons in LFP is as high as 2 eV, which is basically an insulator. This makes the low electron conductivity and ion mobility the main problems affecting its commercial application. Summary of the Invention

[0005] The purpose of this invention is to provide a high-performance lithium manganese iron phosphate cathode material, its preparation method, and a lithium-ion battery. This lithium manganese iron phosphate cathode material is an MXene-doped carbon-coated lithium manganese iron phosphate composite material (abbreviated as LMFP / C@MXene composite material). During the high-temperature calcination of the lithium manganese iron phosphate cathode material, polyethylene terephthalate (PET) serves as a carbon source, enabling the lithium manganese iron phosphate to be coated and acting as a connector, allowing the lithium manganese iron phosphate particles to grow on the surface of MXene nanosheets, forming a three-dimensional porous hierarchical conductive network structure. This improves the material's conductivity, capacitance, and rate performance, and further enhances its low-temperature performance.

[0006] To achieve the above objectives, the present invention adopts the following technical solution:

[0007] In a first aspect, the present invention provides a method for preparing a lithium manganese iron phosphate cathode material, comprising the following steps:

[0008] S1. Activate single-layer or few-layer MXene two-dimensional materials to remove residual groups on the surface and obtain MXene nanosheets;

[0009] S2. React the system of dimethyl benzoate, ethylene glycol and lithium manganese iron phosphate precursor to generate polyethylene terephthalate and coat the lithium manganese iron phosphate precursor.

[0010] S3. After uniformly mixing the MXene nanosheets obtained in step S1 and the polyethylene terephthalate-coated lithium manganese iron phosphate precursor obtained in step S2, heat treatment is performed to obtain the lithium manganese iron phosphate cathode material.

[0011] In the above-mentioned method for preparing lithium manganese iron phosphate cathode material, the MXene two-dimensional material is Ti3C2T. x Ti2CT x Mo3CT x Nb2CT x and V2CT x At least one of them;

[0012] The thickness of the single-layer or few-layer MXene two-dimensional material can be 2 to 10 nm, specifically 5 nm;

[0013] The sheet diameter of the single-layer or few-layer MXene two-dimensional material is 200nm to 2μm, such as an average sheet diameter of 500nm.

[0014] In the above-mentioned method for preparing lithium manganese iron phosphate cathode material, the activation treatment includes: dispersing the monolayer or few-layer MXene two-dimensional material in an aqueous ammonia solution for hydrothermal reaction, and washing and drying after the reaction is completed;

[0015] 0.5g of the monolayer or few-layer MXene two-dimensional material is dispersed in 100mL of the aqueous solution of ammonia;

[0016] The aqueous solution of ammonia consists of water in a volume ratio of (4-5):1 and ammonia solution with a mass concentration of 20%.

[0017] The temperature of the hydrothermal reaction can be 180–240°C, such as 180°C, and the time can be 1–3 hours, such as 2 hours.

[0018] The drying process can specifically involve vacuum drying at 80°C for 6 hours.

[0019] In the above-mentioned method for preparing lithium manganese iron phosphate cathode material, the preparation of the lithium manganese iron phosphate precursor includes:

[0020] S21. Dissolve the iron source, manganese source and phosphorus source in water and mix well. Add an organic solvent to obtain the first mixture.

[0021] S22. An aqueous solution of lithium source is added dropwise to the first mixture. After the addition is complete, the mixture is reacted under an inert atmosphere to obtain the lithium manganese iron phosphate precursor.

[0022] In the above-mentioned method for preparing lithium manganese iron phosphate cathode material, the iron source can be one or more of ferrous oxalate, ferrous sulfate, ferrous nitrate, ferrous phosphate, and ferrous carbonate.

[0023] The manganese source may be one or more of manganese acetate, manganese nitrate, manganese sulfate, manganese carbonate, and manganese chloride;

[0024] The phosphorus source may be one or more of phosphoric acid, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, potassium dihydrogen phosphate, potassium monohydrogen phosphate, sodium dihydrogen phosphate, and sodium monohydrogen phosphate.

[0025] The lithium source may be one or more of lithium hydroxide, lithium carbonate, lithium nitrate, lithium sulfate, lithium chloride, lithium phosphate, and lithium acetate.

[0026] The molar ratio of the iron source, the manganese source, the phosphorus source, and the lithium source can be (0.4–0.35):(0.6–0.65):1:3, such as 0.4:0.6:1:3;

[0027] The organic solvent may be dimethyl sulfoxide or N-methylpyrrolidone;

[0028] The reaction temperature in step S22 can be 120-180℃, specifically 120℃, and the reaction time can be 24-36h, specifically 24h.

[0029] In the above-mentioned method for preparing lithium iron manganese phosphate cathode material, the mass ratio of dimethyl terephthalate, ethylene glycol and lithium iron manganese phosphate precursor is 2.5:1:(80-100), such as 2.5:1:90, 2.5:1:100 or 2.5:1:(90-100).

[0030] The reaction in step S2 includes: heating the system to 130–180°C and holding it for 1 hour under stirring and inert gas conditions, such as 160°C, and then heating it to 240–280°C and holding it for 3–4 hours, such as 250°C and holding it for 3 hours. It is understood that the reaction in step S2 is followed by: filtering, washing, and drying the product obtained from the reaction, and collecting the product. Specifically, the drying can be vacuum drying at 80°C for 6 hours.

[0031] In the above-mentioned method for preparing lithium manganese iron phosphate cathode material, the mass ratio of the polyethylene terephthalate-coated lithium manganese iron phosphate precursor to the MXene nanosheets is (20-35):1, such as 20:1 or 35:1.

[0032] The heat treatment is carried out in an inert atmosphere, with a heating rate of 3℃ / min, a holding temperature of 600~800℃, such as 700℃, and a holding time of 4~10h, such as 5h.

[0033] The inert atmosphere can be nitrogen, argon, or a mixture of nitrogen and argon.

[0034] In the above-mentioned method for preparing lithium manganese iron phosphate cathode material, the mixing step in step S3 includes:

[0035] S31. Mix the aqueous dispersion of the polyethylene terephthalate-coated lithium manganese iron phosphate precursor and the aqueous dispersion of the MXene nanosheets, stir for 4 to 12 hours, and separate the solid material.

[0036] S32. The solid material is vacuum dried at a temperature of 80-120°C for 6-12 hours.

[0037] The specific mass concentration of the aqueous dispersion of the polyethylene terephthalate-coated lithium manganese iron phosphate precursor can be 30%.

[0038] The concentration of the aqueous dispersion of the MXene nanosheets can be 25 mg / mL.

[0039] The stirring time can specifically be 5 hours;

[0040] The vacuum drying temperature can be 80℃, and the drying time can be 12 hours.

[0041] Secondly, the present invention provides a lithium manganese iron phosphate cathode material obtained by any of the preparation methods described above.

[0042] Thirdly, the present invention provides a lithium-ion battery, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the active material in the positive electrode is the lithium manganese iron phosphate positive electrode material.

[0043] Compared with the prior art, the present invention has the following advantages: it provides an MXene-modified carbon-coated lithium manganese iron phosphate material and its preparation method. The electronic conductivity, rate performance and low-temperature performance of the material can be effectively improved by polyethylene terephthalate coating and MXene modification followed by heat treatment.

[0044] (1) The present invention first synthesizes a precursor of lithium manganese iron phosphate, which can ensure the stability of the synthesized lithium manganese iron phosphate and maintain its activity. Then, through the polycondensation reaction of polyethylene terephthalate, a coating layer is introduced, which can further improve the ionic conductivity of lithium-ion conductor while stabilizing the lithium manganese iron phosphate material.

[0045] (2) Polyethylene terephthalate (PET) serves as a carbon source, enabling the coating of lithium manganese iron phosphate (LFP) and acting as a connector to allow LFP particles to grow on the surface of MXene nanosheets, forming a three-dimensional porous hierarchical conductive network structure. This three-dimensional porous hierarchical LFP composite material significantly improves the material's conductivity. Simultaneously, the hierarchical network structure provides channels for lithium ion diffusion, ensuring sufficient contact with the electrolyte and enhancing the material's rate capability and low-temperature performance.

[0046] (3) The anchoring effect of the polymerization reaction by using polyethylene terephthalate as a carbon source alleviates the agglomeration and volume increase of LMFP nanoparticles, and further improves the capacitance and rate performance of the material. Attached Figure Description

[0047] Figure 1 The scanning electron microscope (SEM) results are for the lithium manganese iron phosphate cathode material prepared in Example 1 of this invention. Detailed Implementation

[0048] The present invention will now be described in further detail with reference to specific embodiments. The given embodiments are merely illustrative of the invention and not intended to limit its scope. The embodiments provided below can serve as a guide for further improvements by those skilled in the art and do not constitute a limitation on the invention in any way.

[0049] Unless otherwise specified, the experimental methods used in the following examples are conventional methods; and the materials and reagents used are commercially available unless otherwise specified.

[0050] The MXene two-dimensional materials used in the following examples were purchased from Beijing Beike New Materials Technology Co., Ltd., and the product names are Ti2CT single / few-layer powder materials, respectively. x Single / few-layer powder materials Ti3C2T x The product numbers are BK2020040403 and BK2020040406 respectively.

[0051] Example 1: Preparation of MXene-modified carbon-coated lithium manganese iron phosphate composite material

[0052] The MXene-modified carbon-coated lithium manganese iron phosphate composite material was prepared according to the following steps:

[0053] S1 and MXene two-dimensional material processing and preparation:

[0054] The purchased Ti2CT has a thickness of 5nm and an average wafer diameter of 500nm. x 0.5g of powder was dispersed in an ammonia solution consisting of 80ml of deionized water and 20ml of 20% ammonia solution. The solution was placed in a reaction vessel and hydrothermally reacted at 180℃ for 2h. The resulting dispersion was washed with deionized water by centrifugation and then vacuum dried at 80℃ for 6h to obtain MXene nanosheets.

[0055] S2. Preparation of lithium manganese iron phosphate precursor: Weigh 5.84g FeSO4·7H2O, 8.7g MnSO4·4H2O, and 6.92g phosphoric acid and dissolve them in 500mL deionized water. After stirring and mixing evenly, add 500mL DMSO to the reaction flask. Weigh 7.55g LiOH·H2O and dissolve it in 200mL deionized water. Add the LiOH aqueous solution dropwise to the above mixed solution of FeSO4, MnSO4, and phosphoric acid under a nitrogen atmosphere. After the addition is complete, react under a nitrogen atmosphere at 120℃ for 24h. After cooling to room temperature, filter and wash to obtain a yellowish-brown filter cake.

[0056] S3, polyethylene terephthalate-coated lithium manganese iron phosphate precursor: A certain amount (5g) of filter cake prepared by dimethyl terephthalate, ethylene glycol and S2 was added as reactants to a three-necked flask. The mass ratio of dimethyl terephthalate: ethylene glycol: lithium manganese iron phosphate precursor was 2.5:1:90. The reactants were heated to 160℃ and kept under stirring and nitrogen for 1 hour. The temperature was then raised to 250℃ and kept under nitrogen for 3 hours. The mixture was then filtered, washed, and vacuum dried at 80℃ for 6 hours to obtain a powder.

[0057] S4. The LMFP precursor coated after reaction S3 was redispersed in deionized water at a mass ratio of 30 wt%. 25 mg / ml MXene aqueous dispersion was added at a mass ratio of LMFP precursor:MXene = 20:1. After stirring for 5 h, the product was collected by vacuum filtration and dried in a vacuum oven at 80 °C for 12 h. The mixed product was placed in a tube furnace and subjected to high-temperature treatment under a nitrogen atmosphere at a temperature rise of 3 °C / min, a sintering temperature of 700 °C, and a sintering time of 5 h to obtain the LMFP / C@MXene composite material.

[0058] Scanning electron microscope images of the cathode material obtained in this embodiment are as follows: Figure 1 As shown. By Figure 1 It can be seen that the granular lithium manganese iron phosphate is coated with carbon, and MXene nanosheets play a connecting role in it.

[0059] Example 2: Preparation of MXene-modified carbon-coated lithium manganese iron phosphate composite material

[0060] The MXene-modified carbon-coated lithium manganese iron phosphate composite material was prepared according to the following steps:

[0061] S1 and MXene two-dimensional material processing and preparation:

[0062] We will acquire Ti2CT with a thickness of 5nm and an average wafer diameter of 500nm. x Powder and Ti3C2T x 0.25 g of each powder was dispersed in an ammonia solution consisting of 80 ml of deionized water and 20 ml of 20% ammonia solution. The mixture was placed in a reaction vessel and hydrothermally reacted at 180 °C for 2 h. The resulting dispersion was washed with deionized water by centrifugation and then vacuum dried at 80 °C for 6 h to obtain MXene nanosheets.

[0063] S2. Preparation of lithium manganese iron phosphate precursor: Weigh 5.84g FeSO4·7H2O, 8.7g MnSO4·4H2O, and 6.92g phosphoric acid and dissolve them in 500mL deionized water. After stirring and mixing evenly, add 500mL DMSO to the reaction flask. Weigh 7.55g LiOH·H2O and dissolve it in 200mL deionized water. Add the LiOH aqueous solution dropwise to the above mixed solution of FeSO4, MnSO4, and phosphoric acid under a nitrogen atmosphere. After the addition is complete, react under a nitrogen atmosphere at 120℃ for 24h. After cooling to room temperature, filter and wash to obtain a yellowish-brown filter cake.

[0064] S3, polyethylene terephthalate-coated lithium manganese iron phosphate precursor: A certain amount (5g) of filter cake prepared by dimethyl terephthalate, ethylene glycol and S2 was added as reactants to a three-necked flask. The mass ratio of dimethyl terephthalate: ethylene glycol: lithium manganese iron phosphate precursor was 2.5:1:100. The reactants were heated to 160℃ and kept under stirring and nitrogen drying conditions for 1 hour. The mixture was then heated to 250℃ and kept under nitrogen conditions for 3 hours. After filtration and washing, the mixture was vacuum dried at 80℃ for 6 hours to obtain a powder.

[0065] S4. The LMFP precursor coated after reaction S3 was redispersed in deionized water at a mass ratio of 30 wt%. 25 mg / ml MXene aqueous dispersion was added at a mass ratio of LMFP precursor to MXene of 35:1. After stirring for 5 h, the product was collected by vacuum filtration and dried in a vacuum oven at 80 °C for 12 h. The mixed product was placed in a tube furnace and subjected to high-temperature treatment under a nitrogen atmosphere at a temperature rise of 3 °C / min, a sintering temperature of 700 °C, and a sintering time of 5 h to obtain the LMFP / C@MXene composite material.

[0066] Comparative Example 1

[0067] LiMnFePO4 / C was prepared according to the following steps:

[0068] S2. Preparation of lithium manganese iron phosphate precursor: Weigh 5.84g FeSO4·7H2O, 8.7g MnSO4·4H2O, and 6.92g phosphoric acid and dissolve them in 500mL deionized water. After stirring and mixing evenly, add 500mL DMSO to the reaction flask. Weigh 7.55g LiOH·H2O and dissolve it in 200mL deionized water. Add the LiOH aqueous solution dropwise to the above mixed solution of FeSO4, MnSO4, and phosphoric acid under a nitrogen atmosphere. After the addition is complete, react under a nitrogen atmosphere at 120℃ for 24h. After cooling to room temperature, filter and wash to obtain a yellowish-brown filter cake.

[0069] S3, polyethylene terephthalate-coated lithium manganese iron phosphate precursor: A certain amount (5g) of filter cake prepared by dimethyl terephthalate, ethylene glycol and S2 was added as reactants to a three-necked flask. The mass ratio of dimethyl terephthalate: ethylene glycol: lithium manganese iron phosphate precursor was 2.5:1:100. The reactants were heated to 160℃ and kept under stirring and nitrogen drying conditions for 1 hour. The mixture was then heated to 250℃ and kept under nitrogen conditions for 3 hours. After filtration and washing, the mixture was vacuum dried at 80℃ for 6 hours to obtain a powder.

[0070] S4. The LMFP precursor coated after reaction S3 is redispersed in deionized water at a mass ratio of 30 wt%. After stirring for 5 h, the product is collected by vacuum filtration and dried in a vacuum oven at 80 °C for 12 h. The mixed product is placed in a tube furnace and treated at high temperature under a nitrogen atmosphere at a temperature rise of 3 °C / min, a sintering temperature of 700 °C, and a sintering time of 5 h to obtain the LMFP / C composite material.

[0071] Comparative Example 2

[0072] The preparation was carried out according to the steps in Example 1, except that the activation of the MXene two-dimensional material was omitted. The specific steps are as follows:

[0073] S1. Directly use purchased Ti2CT with a thickness of 5nm and an average wafer diameter of 500nm. x Powder, as MXene nanosheets;

[0074] S2. Preparation of lithium manganese iron phosphate precursor: Weigh 5.84g FeSO4·7H2O, 8.7g MnSO4·4H2O, and 6.92g phosphoric acid and dissolve them in 500mL deionized water. After stirring and mixing evenly, add 500mL DMSO to the reaction flask. Weigh 7.55g LiOH·H2O and dissolve it in 200mL deionized water. Add the LiOH aqueous solution dropwise to the above mixed solution of FeSO4, MnSO4, and phosphoric acid under a nitrogen atmosphere. After the addition is complete, react under a nitrogen atmosphere at 120℃ for 24h. After cooling to room temperature, filter and wash to obtain a yellowish-brown filter cake.

[0075] S3, polyethylene terephthalate-coated lithium manganese iron phosphate precursor: A certain amount (5g) of filter cake prepared by dimethyl terephthalate, ethylene glycol and S2 was added to a three-necked flask as reactants. The mass ratio of dimethyl terephthalate: ethylene glycol: lithium manganese iron phosphate precursor was 2.5:1:90. The reactants were heated to 160℃ and kept under stirring and nitrogen for 1 hour. The mixture was then heated to 250℃ and kept under nitrogen for 3 hours. After filtration and washing, the mixture was vacuum dried at 80℃ for 6 hours to obtain a powder.

[0076] S4. The LMFP precursor coated after reaction S3 was redispersed in deionized water at a mass ratio of 30 wt%. 25 mg / ml MXene aqueous dispersion was added at a mass ratio of LMFP precursor:MXene = 20:1. After stirring for 5 h, the product was collected by vacuum filtration and dried in a vacuum oven at 80 °C for 12 h. The mixed product was placed in a tube furnace and subjected to high-temperature treatment under a nitrogen atmosphere at a temperature rise of 3 °C / min, a sintering temperature of 700 °C, and a sintering time of 5 h to obtain the LMFP / C@MXene composite material (unactivated).

[0077] Comparative Example 3

[0078] Prepared according to the steps in Example 1, except that the carbon source is replaced with glucose. The specific steps are as follows:

[0079] S1 and MXene two-dimensional material processing and preparation:

[0080] We will acquire T with a thickness of 5nm and an average wafer diameter of 500nm. i2 CT x 0.5g of powder was dispersed in an ammonia solution consisting of 80ml of deionized water and 20ml of 20% ammonia solution. The solution was placed in a reaction vessel and hydrothermally reacted at 180℃ for 2h. The resulting dispersion was washed with deionized water by centrifugation and then vacuum dried at 80℃ for 6h to obtain MXene nanosheets.

[0081] S2. Preparation of lithium manganese iron phosphate precursor: Weigh 5.84g FeSO4·7H2O, 8.7g MnSO4·4H2O, and 6.92g phosphoric acid and dissolve them in 500mL deionized water. After stirring and mixing evenly, add 500mL DMSO to the reaction flask. Weigh 7.55g LiOH·H2O and dissolve it in 200mL deionized water. Add the LiOH aqueous solution dropwise to the above mixed solution of FeSO4, MnSO4, and phosphoric acid under a nitrogen atmosphere. After the addition is complete, react under a nitrogen atmosphere at 120℃ for 24h. After cooling to room temperature, filter and wash to obtain a yellowish-brown filter cake.

[0082] S3, Lithium manganese iron phosphate precursor with added glucose: A certain amount (5g) of filter cake prepared by glucose and S2 was added to a three-necked flask. The mass ratio of glucose to lithium manganese iron phosphate precursor was 3.5:100. The reactants were heated to 160°C and kept under stirring and nitrogen flow drying conditions for 1 hour. The mixture was then heated to 250°C and kept under nitrogen conditions for 3 hours. After filtration and washing, the mixture was vacuum dried at 80°C for 6 hours to obtain a powder.

[0083] S4. The LMFP precursor coated after reaction S3 was redispersed in deionized water at a mass ratio of 30 wt%. 25 mg / ml MXene aqueous dispersion was added at a mass ratio of LMFP precursor:MXene = 20:1. After stirring for 5 h, the product was collected by vacuum filtration and dried in a vacuum oven at 80 °C for 12 h. The mixed product was placed in a tube furnace and subjected to high-temperature treatment under a nitrogen atmosphere at a temperature rise of 3 °C / min, a sintering temperature of 700 °C, and a sintering time of 5 h to obtain the LMFP / C@MXene composite material.

[0084] Electrochemical performance testing:

[0085] The positive electrode materials prepared in the above examples and comparative examples were assembled into CR2016 coin cells, wherein: the negative electrode is a lithium metal sheet, the separator is a polypropylene membrane (PP membrane), and the electrolyte solution is 1M LiPF6 in EC / DMC (1:1, vol%). Electrochemical performance was tested at current densities of 0.2C, 1C, 2C, and 5C, and a low-temperature test was performed at -20°C to determine its rate capability and low-temperature performance.

[0086] The experimental results are shown in Table 1.

[0087] Table 1. Electrochemical performance test results

[0088]

[0089] As can be seen from Table 1, the cathode material of the present invention can improve the conductivity of lithium manganese iron phosphate cathode material, enhance the capacitance and rate performance of the material, and further improve the low-temperature performance of the material.

[0090] The present invention has been described in detail above. Those skilled in the art will recognize that the invention can be practiced in a wide range of ways with equivalent parameters, concentrations, and conditions without departing from its spirit and scope. While specific embodiments have been provided, it should be understood that further modifications can be made to the invention. In summary, according to the principles of the invention, this application is intended to include any changes, uses, or improvements to the invention, including modifications made using conventional techniques known in the art that depart from the scope disclosed herein.

Claims

1. A method for preparing a lithium manganese iron phosphate cathode material, characterized in that, Includes the following steps: S1. Activate single-layer or few-layer MXene two-dimensional materials to remove residual groups on the surface and obtain MXene nanosheets; S2. React the system of dimethyl terephthalate, ethylene glycol and lithium manganese iron phosphate precursor to generate polyethylene terephthalate and coat the lithium manganese iron phosphate precursor. The mass ratio of the dimethyl terephthalate, the ethylene glycol, and the lithium iron manganese phosphate precursor is 2.5:1:(80~100). The reaction described in step S2 includes: heating the system to 130~180°C and holding it for 1 hour under stirring and inert gas conditions, and then heating it to 240~280°C and holding it for 3~4 hours; S3. After uniformly mixing the MXene nanosheets obtained in step S1 and the polyethylene terephthalate-coated lithium manganese iron phosphate precursor obtained in step S2, heat treatment is performed to obtain the lithium manganese iron phosphate cathode material. The mass ratio of the polyethylene terephthalate-coated lithium manganese iron phosphate precursor to the MXene nanosheets is (20~35):1; The heat treatment is carried out under an inert atmosphere, with a heating rate of 3℃ / min, a holding temperature of 600~800℃, and a holding time of 4~10 h.

2. The method for preparing lithium manganese iron phosphate cathode material according to claim 1, characterized in that: The MXene two-dimensional material is Ti3C2T. x Ti2CT x Mo3CT x Nb2CT x and V2CT x At least one of them; The thickness of the single-layer or few-layer MXene two-dimensional material is 2~10nm; The sheet diameter of the single-layer or few-layer MXene two-dimensional material is 200 nm to 2 μm.

3. The method for preparing lithium manganese iron phosphate cathode material according to claim 1 or 2, characterized in that: The activation treatment includes: dispersing the monolayer or few-layer MXene two-dimensional material in an aqueous ammonia solution for a hydrothermal reaction, followed by washing with water and drying after the reaction is complete; 0.5g of the monolayer or few-layer MXene two-dimensional material is dispersed in 100mL of the aqueous solution of ammonia; The aqueous ammonia solution is composed of water in a volume ratio of (4~5):1 and ammonia solution with a mass concentration of 20%. The hydrothermal reaction is carried out at a temperature of 180~240℃ for 1~3 hours.

4. The method for preparing lithium manganese iron phosphate cathode material according to claim 1 or 2, characterized in that: The preparation of the lithium manganese iron phosphate precursor includes: S21. Dissolve the iron source, manganese source and phosphorus source in water and mix well. Add an organic solvent to obtain the first mixture. S22. An aqueous solution of lithium source is added dropwise to the first mixture. After the addition is complete, the mixture is reacted under an inert atmosphere to obtain the lithium manganese iron phosphate precursor.

5. The method for preparing lithium manganese iron phosphate cathode material according to claim 4, characterized in that: The iron source is one or more of ferrous oxalate, ferrous sulfate, ferrous nitrate, ferrous phosphate, and ferrous carbonate. The manganese source is one or more of manganese acetate, manganese nitrate, manganese sulfate, manganese carbonate, and manganese chloride; The phosphorus source is one or more of phosphoric acid, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate, potassium dihydrogen phosphate, potassium monohydrogen phosphate, sodium dihydrogen phosphate, and sodium monohydrogen phosphate. The lithium source is one or more of lithium hydroxide, lithium carbonate, lithium nitrate, lithium sulfate, lithium chloride, lithium phosphate, and lithium acetate. The molar ratio of the iron source, the manganese source, the phosphorus source, and the lithium source is (0.4~0.35):(0.6~0.65):1:3; The organic solvent is dimethyl sulfoxide or N-methylpyrrolidone; The reaction in step S22 is carried out at a temperature of 120~180℃ for 24~36h.

6. The method for preparing lithium manganese iron phosphate cathode material according to claim 1 or 2, characterized in that: The mixing step in step S3 includes: S31. Mix the aqueous dispersion of the polyethylene terephthalate-coated lithium manganese iron phosphate precursor and the aqueous dispersion of the MXene nanosheets, stir for 4-12 hours, and separate the solid material. S32. The solid material is vacuum dried at a temperature of 80~120℃ for 6~12 hours.

7. The lithium manganese iron phosphate cathode material obtained by the preparation method according to any one of claims 1-6.

8. A lithium-ion battery, characterized in that, It includes a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the active material in the positive electrode is the lithium manganese iron phosphate positive electrode material as described in claim 7.

Citation Information

Patent Citations

  • Preparation method of conductive modified lithium iron phosphate

    CN102683698A

  • Method for intercalating and stripping two-dimensional crystal titanium carbide nano material by using ammonia water

    CN106185936A

  • Preparation method of LiFePO4 (at) C / MXene composite material

    CN112490426A

  • Lithium ion battery positive electrode material and preparation method thereof

    CN114335469A