Preparation method of bamboo charcoal cotton fiber electromagnetic shielding composite material
Bamboo charcoal cotton fiber electromagnetic shielding composite material was prepared by a sodium hydroxide-urea low-temperature micro-dissolution-blending process, which solved the environmental protection and cost problems of traditional electromagnetic shielding materials, and realized efficient electromagnetic shielding and high-value utilization of biomass resources. It is suitable for civilian and industrial electronic equipment.
Patent Information
- Application Number
- CN202311317687.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-11
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-10-11
AI Technical Summary
Existing electromagnetic shielding materials suffer from problems such as environmentally unfriendly raw materials, high costs, and difficult processing, and there is limited research on traditional biomass electromagnetic shielding materials.
Bamboo charcoal and cotton fiber electromagnetic shielding composite materials were prepared using a sodium hydroxide-urea low-temperature micro-dissolution-blending process to form a core-shell structure. By utilizing the blending process of bamboo charcoal and cotton fiber, an all-biomass electromagnetic shielding material was prepared.
It achieves green, environmentally friendly, and low-cost electromagnetic shielding, with excellent electrical conductivity and electromagnetic shielding effectiveness, promoting the high-value utilization of bamboo and cotton fibers, and is suitable for civilian and industrial electronic equipment.
Smart Images

Figure CN117580346B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electromagnetic shielding materials technology, specifically a method for preparing a bamboo charcoal cotton fiber electromagnetic shielding composite material. Background Technology
[0002] The rapid development of electronic information technology has brought great convenience to people's lives and work, but it has also brought increasingly serious electromagnetic pollution. Electromagnetic pollution has become the fourth largest form of pollution after water pollution, air pollution, and noise pollution. It not only interferes with the normal operation of surrounding electronic equipment, but also causes unpredictable harm to human health through thermal, non-thermal, and cumulative effects. It can even lead to the leakage of important information, threatening national security. Therefore, the development of a new type of high-performance electromagnetic shielding material is of great significance for the prevention and control of electromagnetic pollution.
[0003] According to domestic and international research, electromagnetic shielding materials can be divided into two main categories: metallic shielding materials and polymer shielding materials. While pure metallic shielding materials possess excellent shielding performance, their shortcomings are obvious and their performance is limited, failing to meet the performance requirements of most fields. The fabrication of shielding materials using fillers or thin layers is a key development direction for metallic shielding materials. For example, Xu Wenzheng et al. used DC magnetron sputtering technology to prepare polyester nonwoven fabrics with surface-deposited Ag films, achieving a shielding effectiveness of 39.37 dB. Although these metallic shielding materials compensate for some of the shortcomings of pure metallic materials, they still suffer from drawbacks such as bulkiness, susceptibility to corrosion, high cost, and difficult processing, and are gradually being replaced by newer shielding materials in recent years. Compared to metallic shielding materials, polymer shielding materials have advantages such as low density, corrosion resistance, and adjustable conductivity, making them the most promising alternative to metallic shielding materials. Based on different raw materials and preparation methods, polymer shielding materials can be further divided into intrinsically conductive shielding materials and filled composite shielding materials. In recent years, intrinsically conductive shielding materials have attracted widespread research attention. For example, Lee et al. prepared polyvinylidene fluoride-polyethylene dioxythiophene composite nanofibers using chemical polymerization, achieving a shielding effectiveness of 40 dB in the X-band. However, these materials generally suffer from drawbacks such as processing difficulties and lower conductivity compared to metallic materials, remaining somewhat distant from practical applications. Li et al. prepared graphene / styrene-butadiene rubber nanocomposites using spray drying, achieving a shielding effectiveness of 45 dB in the X-band. Compared to intrinsically conductive shielding materials, these carbon-based filled composite shielding materials offer advantages such as low cost and ease of molding, making them a research hotspot in polymer shielding materials. However, it is worth noting that most current electromagnetic shielding materials use non-renewable resources as raw materials, which is detrimental to resource conservation and environmental protection.
[0004] Biomass is an abundant renewable resource with the potential to replace non-renewable resources such as metals, coal, and oil in many fields. Its use in the preparation of electromagnetic shielding materials can not only effectively prevent electromagnetic pollution but also facilitate the high-value utilization of biomass. In recent years, some scholars have conducted research on biomass electromagnetic shielding materials and achieved certain results. For example, Zhang Long et al. first prepared cotton fiber@polyaniline composite materials using in-situ polymerization, and then obtained magnetic cotton fiber@polyaniline composite materials through the physical adsorption of Fe3O4 nanoparticles. The minimum reflection loss of this material was -18.57 dB. Li Xiaoqing et al. prepared bamboo charcoal / high-density polyethylene composite materials through melt extrusion-molding, achieving a shielding effectiveness of 33.7 dB in the X-band. Although biomass electromagnetic shielding materials have attracted attention, research on all-biomass electromagnetic shielding materials is still relatively limited.
[0005] Therefore, inventing a green, environmentally friendly, low-cost, simple-process, and high-performance all-biomass electromagnetic shielding composite material is of great significance in the field of electromagnetic shielding materials. Summary of the Invention
[0006] The purpose of this section is to outline some aspects of the embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.
[0007] Therefore, the purpose of this invention is to provide a method for preparing a bamboo charcoal cotton fiber electromagnetic shielding composite material. The material obtained can not only effectively prevent and control electromagnetic pollution and secondary pollution, but also solve the problem of the environmentally unfriendly raw materials of traditional electromagnetic shielding materials, which is conducive to realizing the high-value utilization of bamboo and cotton fibers.
[0008] To address the aforementioned technical problems, according to one aspect of the present invention, the present invention provides the following technical solution: A method for preparing a bamboo charcoal cotton fiber electromagnetic shielding composite material, comprising: S1. Sodium hydroxide, urea and deionized water are added to a glass container in a certain mass ratio and stirred thoroughly to obtain a uniform sodium hydroxide-urea low-temperature solution. S2. Add the bamboo charcoal carbonized at 1600℃ to the low-temperature dissolving solution, then disperse it by ultrasonication, and then stir it thoroughly. Finally, put the mixture into the refrigerator's crisper compartment to pre-cool it to obtain a pre-cooled mixture. S3. Dry the cotton fibers, then add them to the pre-cooled blending liquid, and then use a stepless speed-regulating stirrer to stir at high speed to obtain a uniformly mixed mixture. S4. Fill the mold evenly with the mixture, then use a circulating water multi-purpose vacuum pump to defoam it. Then put the defoamed mixture into the freezer compartment of the refrigerator to obtain a gelled mixture. S5. After washing the hydrogel with deionized water until neutral, place it in a hot press to dry it thoroughly to obtain the electromagnetic shielding composite material with a core-shell structure.
[0009] In a preferred embodiment of the preparation method of the bamboo charcoal cotton fiber electromagnetic shielding composite material of the present invention, in step S1, the mass ratio of sodium hydroxide, urea and deionized water is 5-10:10-15:75-85.
[0010] In a preferred embodiment of the preparation method of the bamboo charcoal cotton fiber electromagnetic shielding composite material of the present invention, in step S2, the amount of bamboo charcoal added is 10-30% of the mass fraction of the composite material.
[0011] In a preferred embodiment of the preparation method of the bamboo charcoal cotton fiber electromagnetic shielding composite material of the present invention, in step S2, the pre-cooling temperature is 2-8℃ and the pre-cooling time is 10-60 min.
[0012] In a preferred embodiment of the preparation method of the bamboo charcoal cotton fiber electromagnetic shielding composite material of the present invention, in step S3, the mass ratio of the oven-dried cotton fiber to the sodium hydroxide-urea low-temperature solution is 1:8-12.
[0013] In a preferred embodiment of the preparation method of the bamboo charcoal cotton fiber electromagnetic shielding composite material of the present invention, in step S3, the stirring speed is 500-1500 r / min and the stirring time is 0.5-2h.
[0014] In a preferred embodiment of the preparation method of the bamboo charcoal cotton fiber electromagnetic shielding composite material of the present invention, in step S4, the vacuum degree is -0.1 MPa and the defoaming time is 0.5-1h.
[0015] In a preferred embodiment of the preparation method of the bamboo charcoal cotton fiber electromagnetic shielding composite material of the present invention, in step S4, the freezing temperature is -10 to -15 ℃ and the freezing time is 4-12 h. In a preferred embodiment of the preparation method of the bamboo charcoal cotton fiber electromagnetic shielding composite material of the present invention, in step S5, the hot pressing temperature is 60-120 ℃, the hot pressing pressure is 0-1 MPa, and the hot pressing time is 12-24 h.
[0016] In a preferred embodiment of the preparation method of the bamboo charcoal cotton fiber electromagnetic shielding composite material of the present invention, in step S5, micron-sized cotton fiber is used as the core, bamboo charcoal as the shell, and nano-sized regenerated fiber is used as the crosslinking agent.
[0017] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention uses abundant and inexpensive bamboo charcoal and cotton fiber as raw materials. A composite hydrogel is prepared by a sodium hydroxide-urea low-temperature micro-dissolution-blending process. After drying, a bamboo charcoal / cotton fiber electromagnetic shielding composite material with a core-shell structure is finally obtained. This invention prepares an all-biomass electromagnetic shielding material with zero chemical crosslinking agent addition. It not only effectively solves the problem of the environmentally unfriendly raw materials of traditional electromagnetic shielding materials, but also greatly promotes the high-value utilization of these two biomasses.
[0018] 2. The preparation process of this invention is simple and has low production cost, and has great potential for large-scale production. The developed green and environmentally friendly sodium hydroxide-urea low-temperature micro-dissolution-blending process can destroy some of the hydrogen bond bonds between cotton fibers while retaining most of the micron-sized cotton fibers. The resulting large number of nano-sized regenerated fibers can tightly coat bamboo charcoal on the surface of micron-sized cotton fibers through a densely entangled network structure. Under further drying and shrinkage, a core-shell structure with micron-sized cotton fibers as the core and bamboo charcoal as the shell is formed.
[0019] 3. The electromagnetic shielding composite material prepared by this invention has excellent comprehensive performance. The core-shell structure facilitates the selective dispersion and adhesion of bamboo charcoal with abundant pore structure and large specific surface area to the surface of cotton fibers, providing a shell path for rapid electron transport. This results in excellent electrical conductivity (0.48 S / cm) and excellent electromagnetic shielding effectiveness (51.5 dB) mainly based on absorption and attenuation. In addition, the flexural strength and flexural modulus of this material can reach 78.1 MPa and 3.7 GPa, respectively. It also has excellent thermal properties and biodegradability, and has great application potential in the fields of civilian and industrial electronic equipment. Attached Figure Description
[0020] To more clearly illustrate the technical solutions of the embodiments of the present invention, the present invention will be described in detail below with reference to the accompanying drawings and detailed embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein: Figure 1 This is a process flow diagram for preparing a bamboo charcoal / cotton fiber electromagnetic shielding composite material according to the present invention; Figure 2 This is a scanning electron microscope image of the cross-section of the composite material in Embodiment 1 of the present invention; Figure 3 This is an optical microscope image of the composite core-shell structure in Embodiment 1 of the present invention; Figure 4 This is a diagram showing the electromagnetic shielding performance of the composite material in the X-band in Embodiment 1 of the present invention; Figure 5 The diagram shows the electrical conductivity of composite materials with different bamboo charcoal contents in the comparative examples of this invention. Figure 6 This is a graph showing the electromagnetic shielding performance of composite materials with different bamboo charcoal contents in the X-band in the comparative examples of this invention. Detailed Implementation
[0021] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0022] This invention provides a method for preparing a bamboo charcoal cotton fiber electromagnetic shielding composite material. The resulting material can not only effectively prevent and control electromagnetic pollution and secondary pollution, but also solve the problem of the environmentally unfriendly raw materials of traditional electromagnetic shielding materials, which is conducive to realizing the high-value utilization of bamboo and cotton fibers.
[0023] Figure 1 The diagram shown is a flowchart of a method for preparing a bamboo charcoal cotton fiber electromagnetic shielding composite material according to the present invention. The following is in conjunction with... Figure 1 Examples 1-4 provide a detailed description of the preparation method of a bamboo charcoal cotton fiber electromagnetic shielding composite material according to this embodiment. Example 1
[0024] S1. Add sodium hydroxide, urea and deionized water to a glass container in a mass ratio of 7:12:81 and stir thoroughly to obtain a uniform sodium hydroxide-urea low-temperature solution. S2. Add 30% of the bamboo charcoal by mass of the composite material to the low-temperature dissolving solution, then disperse it by ultrasonication, then stir it thoroughly, and finally put the blend into the refrigerator's crisper compartment at 2°C for 10 minutes to pre-cool it and obtain the pre-cooled blend. S3. Dry the cotton fibers and then add them to the pre-cooled blending solution (the mass ratio of oven-dried cotton fibers to sodium hydroxide-urea low-temperature solution is 1:9). Then use a stepless speed-regulating stirrer to stir at 1500 r / min for 1 hour to obtain a uniformly mixed mixture. S4. Fill the mold evenly with the mixture, and then use a circulating water multi-purpose vacuum pump to vacuum defoam it at a vacuum degree of -0.1 MPa for 0.5 hours. Then place the defoamed mixture in the freezer compartment of a refrigerator at -12℃ for 6 hours to obtain a gelled mixture. S5. After washing the hydrogel with deionized water until neutral, dry it in a hot press at 100℃ and 0MPa for 24h to obtain an electromagnetic shielding composite material with micron-sized cotton fiber as the core, bamboo charcoal as the shell, and nano-sized regenerated fiber as the crosslinking agent. Example 2
[0025] S1. Add sodium hydroxide, urea and deionized water to a glass container in a mass ratio of 8:14:78, stir thoroughly to obtain a uniform sodium hydroxide-urea low-temperature solution. S2. Add 30% of the bamboo charcoal by mass of the composite material to the low-temperature dissolving solution, then disperse it by ultrasonication, and then stir it thoroughly. Finally, put the blend into the refrigerator's crisper compartment at 4°C for 20 minutes to pre-cool it and obtain the pre-cooled blend. S3. Dry the cotton fibers and then add them to the pre-cooled blending solution (the mass ratio of oven-dried cotton fibers to sodium hydroxide-urea low-temperature solution is 1:11). Then use a stepless speed-regulating stirrer to stir at 1000 r / min for 2 hours to obtain a uniformly mixed mixture. S4. Fill the mold evenly with the mixture, and then use a circulating water multi-purpose vacuum pump to vacuum defoam it at a vacuum degree of -0.1 MPa for 0.5 h. Then place the defoamed mixture in the freezer compartment of a refrigerator at -10℃ for 12 h to obtain a gelled mixture. S5. After washing the hydrogel with deionized water until neutral, dry it in a hot press at 80℃ and 0MPa for 24h to obtain an electromagnetic shielding composite material with micron-sized cotton fiber as the core, bamboo charcoal as the shell, and nano-sized regenerated fiber as the crosslinking agent. Example 3
[0026] S1. Add sodium hydroxide, urea and deionized water to a glass container in a mass ratio of 6:10:84, stir thoroughly to obtain a uniform sodium hydroxide-urea low-temperature solution. S2. Add 10% of the bamboo charcoal by mass of the composite material to the low-temperature dissolving solution, then disperse it by ultrasonication, then stir it thoroughly, and finally put the blend into the refrigerator's crisper compartment at 3°C for 45 minutes to pre-cool it to obtain the pre-cooled blend. S3. Dry the cotton fibers and then add them to the pre-cooled blending solution (the mass ratio of oven-dried cotton fibers to sodium hydroxide-urea low-temperature solution is 1:11). Then use a stepless speed-regulating stirrer to stir at 800 r / min for 2 hours to obtain a uniformly mixed mixture. S4. Fill the mold evenly with the mixture, then use a circulating water multi-purpose vacuum pump to vacuum defoam it at a vacuum degree of -0.1 MPa for 1 hour. Then place the defoamed mixture in the freezer compartment of a -15℃ refrigerator for 6 hours to obtain a gelled mixture. S5. After washing the hydrogel with deionized water until neutral, dry it in a hot press at 100℃ and 0MPa for 16h to obtain an electromagnetic shielding composite material with micron-sized cotton fiber as the core, bamboo charcoal as the shell, and nano-sized regenerated fiber as the crosslinking agent. Example 4
[0027] S1. Add sodium hydroxide, urea and deionized water to a glass container in a mass ratio of 7:13:80, stir thoroughly to obtain a uniform sodium hydroxide-urea low-temperature solution. S2. Add 25% of the bamboo charcoal by mass of the composite material to the low-temperature dissolving solution, then disperse it by ultrasonication, and then stir it thoroughly. Finally, put the blend into the refrigerator's crisper compartment at 2°C and pre-cool it for 40 minutes to obtain the pre-cooled blend. S3. Dry the cotton fibers and then add them to the pre-cooled blending solution (the mass ratio of oven-dried cotton fibers to sodium hydroxide-urea low-temperature solution is 1:10). Then use a stepless speed-regulating stirrer to stir at 1200 r / min for 1 hour to obtain a uniformly mixed mixture. S4. Fill the mold evenly with the mixture, and then use a circulating water multi-purpose vacuum pump to vacuum defoam it at a vacuum degree of -0.1 MPa for 1 hour. Then place the defoamed mixture in the freezer compartment of a -14℃ refrigerator for 12 hours to obtain a gelled mixture. S5. After washing the hydrogel with deionized water until neutral, dry it in a hot press at 120℃ and 0MPa for 12 hours to obtain an electromagnetic shielding composite material with micron-sized cotton fiber as the core, bamboo charcoal as the shell, and nano-sized regenerated fiber as the crosslinking agent.
[0028] Comparative Example This comparative example is used to verify the effect of bamboo charcoal content on the conductivity and electromagnetic shielding performance of bamboo charcoal / cotton fiber electromagnetic shielding composite material with core-shell structure. Except for the bamboo charcoal addition amount of 10%, 20% and 30% respectively, the other technical methods are the same as those in Example 1. The composite material with bamboo charcoal addition amount of 30% is actually the corresponding example of Example 1.
[0029] Depend on Figure 5 and Figure 6As can be seen, the bamboo charcoal / cotton fiber electromagnetic shielding composite material with 30% bamboo charcoal addition prepared in Example 1 has excellent electrical conductivity (0.48 S / cm) and excellent electromagnetic shielding effectiveness (51.5 dB) mainly based on absorption and attenuation. The electrical conductivity and shielding effectiveness of the shielding material with 10% bamboo charcoal addition prepared in the comparative example are 0.01 S / cm and 19.0 dB, respectively. The electrical conductivity and shielding effectiveness of the shielding material with 20% bamboo charcoal addition prepared in the comparative example are 0.15 S / cm and 41.8 dB, respectively. Therefore, compared with the bamboo charcoal / cotton fiber electromagnetic shielding composite materials with 10% and 20% bamboo charcoal addition prepared in the comparative example, the bamboo charcoal / cotton fiber electromagnetic shielding composite material prepared in Example 1 has higher electrical conductivity and electromagnetic shielding effectiveness, and is more advantageous in preventing and controlling electromagnetic pollution.
[0030] Although the present invention has been described above with reference to embodiments, various modifications can be made and components can be replaced with equivalents without departing from the scope of the invention. In particular, as long as there is no structural conflict, the features in the disclosed embodiments can be combined with each other in any manner. The lack of an exhaustive description of these combinations in this specification is merely for the sake of brevity and resource conservation. Therefore, the present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A method for preparing a bamboo charcoal cotton fiber electromagnetic shielding composite material, characterized in that, include: S1. Sodium hydroxide, urea and deionized water are added to a glass container in a certain mass ratio and stirred thoroughly to obtain a uniform sodium hydroxide-urea low-temperature solution. S2. Add the bamboo charcoal carbonized at 1600℃ to the low-temperature dissolving solution, then disperse it by ultrasonication, and then stir it thoroughly. Finally, put the mixture into the refrigerator's crisper compartment to pre-cool it to obtain a pre-cooled mixture. S3. Dry the cotton fibers, then add them to the pre-cooled blending liquid, and then use a stepless speed-regulating stirrer to stir at high speed to obtain a uniformly mixed mixture. S4. Fill the mold evenly with the mixture, then use a circulating water multi-purpose vacuum pump to defoam it. Then put the defoamed mixture into the freezer compartment of the refrigerator to obtain a gelled mixture. S5. After washing the hydrogel with deionized water until neutral, place it in a hot press to dry it thoroughly to obtain the electromagnetic shielding composite material with a core-shell structure. In step S3, the mass ratio of oven-dried cotton fiber to sodium hydroxide-urea low-temperature solution is 1:8-12, the stirring speed is 500-1500 r / min, and the stirring time is 0.5-2 h. In step S5, micron-sized cotton fiber is used as the core, bamboo charcoal as the shell, and nano-sized regenerated fiber is used as the crosslinking agent.
2. The preparation method of the bamboo charcoal cotton fiber electromagnetic shielding composite material according to claim 1, characterized in that, In step S1, the mass ratio of sodium hydroxide, urea and deionized water is 5-10:10-15:75-85.
3. The preparation method of a bamboo charcoal cotton fiber electromagnetic shielding composite material according to claim 1, characterized in that, In step S2, the amount of bamboo charcoal added is 10-30% of the mass fraction of the composite material.
4. The preparation method of the bamboo charcoal cotton fiber electromagnetic shielding composite material according to claim 1, characterized in that, In step S2, the pre-cooling temperature is 2-8℃ and the pre-cooling time is 10-60 min.
5. The preparation method of a bamboo charcoal cotton fiber electromagnetic shielding composite material according to claim 1, characterized in that, In step S4, the vacuum degree is -0.1 MPa and the defoaming time is 0.5-1 h.
6. The method for preparing a bamboo charcoal cotton fiber electromagnetic shielding composite material according to claim 1, characterized in that, In step S4, the freezing temperature is -10 to -15°C, and the freezing time is 4 to 12 hours.
7. The method for preparing a bamboo charcoal cotton fiber electromagnetic shielding composite material according to claim 1, characterized in that, In step S5, the hot pressing temperature is 60-120 ℃, the hot pressing pressure is 0-1 MPa, and the hot pressing time is 12-24h.
Citation Information
Patent Citations
Bamboo charcoal base electro-magnetic screen composite material and preparation method thereof
CN101451057A
Cellulose / two-dimensional layered material composite hydrogel and preparation method thereof
CN107973920A
Nitrogen-doped bamboo cellulose carbon aerogel electrode material and preparation method thereof
CN111439740A