Coated cutting tool, method of manufacture and use

By preparing multi-layer wear-resistant hard coatings, especially TiCN and α-Al₂O₃ layers, on cutting tools, the problem of insufficient wear resistance and oxidation resistance of cutting tools in ISO P and ISO K steel applications is solved, thereby improving the cutting edge toughness and tool life.

CN117580974BActive Publication Date: 2026-11-24WALTER AG
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202280045822.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-07-02
Filing Date
2022-06-30
Publication Date
2026-11-24
Estimated Expiration
2042-06-30

AI Technical Summary

Technical Problem

Existing cutting tools are insufficient in wear resistance, oxidation resistance and cutting edge toughness in ISO P and ISO K steel applications, especially in continuous and interrupted cutting.

Method used

The coating employs a multi-layer wear-resistant hard coating structure, including a TiCN layer, a Ti or Ti+Al compound bonding layer, and an α-Al₂O₃ layer, which is prepared by chemical vapor deposition (CVD). The TiCN layer has a specific multi-sublayer structure and texture coefficient, which controls the texture and adhesion of the α-Al₂O₃ layer and improves the overall performance of the coating.

Benefits of technology

It improves the wear resistance, oxidation resistance and cutting edge toughness of cutting tools, and extends tool life, especially showing excellent performance in continuous and interrupted cutting of ISO P and ISO K steels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117580974B_ABST
    Figure CN117580974B_ABST
Patent Text Reader

Abstract

This invention relates to a coated cutting tool consisting of a substrate and a multilayer wear-resistant hard coating, and a method for manufacturing the same. The hard coating is deposited by chemical vapor deposition (CVD) and comprises: a TiCN layer having a multilayer structure with alternating C-type and N-type sublayers and an overall fibrous texture characterized by a texture factor TC(4 2 2) in the range of 3.0 to 5.5; an oxygen-containing Ti or Ti+Al compound bonding layer; and an α-Al2O3 layer above the bonding layer having an overall fibrous texture characterized by a texture factor TC(0 0 12) > 5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a coated cutting tool for chip-forming metal processing, the coated cutting tool comprising a substrate and a multilayer wear-resistant hard coating, the layers of the hard coating being deposited by chemical vapor deposition (CVD). Background Technology

[0002] Cutting tools commonly used in metalworking consist of a base body made of cemented carbide, cermet, ceramic, steel, or cubic boron nitride, and a single or multiple layers of wear-resistant hard material coating deposited by CVD or PVD. Specifically, one type of high-performance cutting tool comprises a cemented carbide base body (substrate), a thin base layer of TiC or TiN, a layer of TiCN, in most cases deposited as MT-TiCN (medium-temperature CVD), followed by an α, κ, or mixed α+κ Al₂O₃ layer. It is also known to place a Ti compound or Ti+Al compound bonding layer between the TiCN layer and the Al₂O₃ layer. This bonding layer can be adapted to transfer crystallographic properties from the underlying TiCN layer to the Al₂O₃ layer and can influence the variants, texture, and adhesion of the Al₂O₃ layer. For example, a certain degree of oxidation on the surface of the Ti or Ti+Al compound bonding layer can promote the formation of α-Al₂O₃ preferentially over the κ variant. Examples can be found in US 7,172,807.

[0003] The performance and lifespan of such cutting tools are influenced by a variety of parameters. Some parameters are more or less determined by the desired machining application, such as the workpiece material and the expected cutting operation. However, there is still potential for improvement in the cutting tools themselves, particularly in terms of coating properties and the balance between different parts and layers of the coating, which affects different wear types and improves tool life and cutting performance. Summary of the Invention

[0004] Technical issues

[0005] One object of the present invention is to provide a coated cutting tool, which, particularly for ISO P and ISO K steels, exhibits improved wear resistance and oxidation resistance as well as enhanced cutting edge toughness in continuous and intermittent cutting.

[0006] Technical solution

[0007] This objective has been achieved by providing a coated cutting tool for chip-forming metalworking, comprising a substrate and a multilayer wear-resistant hard coating, the multilayer wear-resistant hard coating comprising:

[0008] a) A TiCN layer having a total thickness of 2 μm to 20 μm.

[0009] The TiCN layer has a multi-sublayer structure with a total of p alternating C-type and N-type sublayers, where p is an even or odd number in the range of 5 to 25, preferably 5 to 12.

[0010] The C-type and N-type sublayers have different stoichiometry for the atomic ratios of carbon and nitrogen, wherein the C-type TiCN sublayer has a C / N ratio in the range of 1.0 ≤ C / N ≤ 2.0, and the N-type TiCN sublayer has a C / N ratio in the range of 0.5 ≤ C / N < 1.0, and wherein the difference between the C / N ratios of adjacent C-type and N-type layers is ≥ 0.2.

[0011] The TiCN layer therein has an overall fiber texture characterized by a texture factor TC(4 2 2) in the range of 3.0 to 5.5, wherein TC(4 2 2) is defined as follows:

[0012]

[0013] in

[0014] I(hkl) = (hkl) XRD intensity of reflection

[0015] I0(hkl) = Standard intensity of standard powder diffraction data according to ICDD PDF card No. 01-071-6059

[0016] n = 7 = the number of reflections used in the calculation, of which the seven (hkl) reflections used are: (11 1), (2 00), (2 2 0), (3 1 1), (3 3 1), (4 2 0) and (4 2 2).

[0017] b) A single-layer or multi-layer oxygen-containing Ti or Ti+Al compound bonding layer, said bonding layer having a total thickness of 0.5 μm to 3 μm above the TiCN layer.

[0018] c) An α-Al₂O₃ layer, located above the bonding layer, having a total thickness of 2 μm to 15 μm.

[0019] The α-Al₂O₃ layer has an overall fibrous texture characterized by a texture factor TC(0 0 12) > 5, where TC(0 0 12) is defined as follows:

[0020]

[0021] in

[0022] I(hkl) = (hkl) XRD intensity of reflection

[0023] I0(hkl) = Standard strength measured on NIST standard powder SRM676a

[0024] n = 8 = the number of reflections used in the calculation, where the eight (hkl) reflections used are: (1 0 4), (1 10), (1 1 3), (0 2 4), (1 1 6), (3 0 0), (0 0 12), and (0 1 14).

[0025] The standard strength has the following values:

[0026] {hkl} {1 0 4} {1 1 0} {1 1 3} {0 2 4} {1 1 6} {3 0 0} {0 0 12} {0 1 14} <![CDATA[I0(h k l)]]> 87.93 37.68 100.00 45.76 92.43 53.93 2.05 5.16

[0027] In the following text, the terms “{2 1 1} texture of the TiCN layer” and “{0 0 1} texture of the α-Al2O3 layer” refer to preferred crystal orientations in polycrystalline layers, where each crystal plane is more frequently oriented parallel to the substrate surface (perpendicular to the growth direction of the layer) compared to random orientations. Preferred crystal orientations were determined by XRD in this paper and are expressed by the texture coefficients of the corresponding (parallel) crystal {42 2} and {0 0 12} planes, the TC (4 2 2) of the TiCN layer, and the TC (0 0 12) of the α-Al2O3 layer, respectively.

[0028] Improving the properties and performance of cutting tools requires consideration of multiple aspects simultaneously. It has been found that controlling the high {0 0 1} texture of the α-Al₂O₃ layer (indicated by a texture factor TC(0 0 12) > 5) is key to high oxidation resistance and resistance to crater wear. Preferably, the texture factor TC(0 0 12) of the α-Al₂O₃ layer is > 6. On the other hand, it has been found that flank wear resistance is strongly influenced by the microstructure and texture of the TiCN layer in the coating sequence. Another essential characteristic of cutting tool performance and tool life is cutting edge toughness; however, this can be limited by the adhesion of the coating at the layer interface. Low adhesion can lead to tool breakage, chipping, and / or spalling, resulting in premature tool failure. Through a specific coating sequence and the properties of each coating, the inventors have discovered a novel coated cutting tool that provides improved cutting edge toughness and flank wear resistance, as well as improved oxidation resistance and resistance to crater wear.

[0029] In the preferred mode of the coated cutting tool of the present invention, the hard coating layer is deposited by chemical vapor deposition (CVD), and the TiCN layer having a multi-sublayer structure is an MT-TiCN layer deposited by MT-CVD at a reaction temperature in the range of 600°C to 900°C. The polycrystalline TiCN layer consists of columnar grains.

[0030] The Ti or Ti+Al compound bonding layer is preferably deposited by HT-CVD at a reaction temperature in the range of 900°C to 1200°C, and the α-Al2O3 layer is also preferably deposited by HT-CVD at a reaction temperature in the range of 900°C to 1200°C.

[0031] It is known that a certain degree of oxidation in the Ti or Ti+Al compound layer beneath the Al2O3 layer can promote the nucleation and subsequent growth of the α-variant preferentially over other variants. However, it has been found that the development and level of the texture of the α-Al2O3 layer are determined not only by the deposition conditions of the Al2O3 layer itself, but also to some extent by the microstructure and crystal orientation of the underlying TiCN layer. Therefore, controlling the TiCN layer is also crucial for controlling the properties of the subsequent α-Al2O3 layer.

[0032] The inventors have recognized that a fine-grained TiCN layer with a high {211} texture promotes controlled nucleation and deposition of a highly {001}-textured α-Al₂O₃ layer and high flank wear resistance of the coating. Therefore, in this first attempt, it will be assumed that the TiCN layer has the highest possible {211} texture to improve the favorable properties resulting from the highly {001}-textured α-Al₂O₃ layer and the high flank wear resistance.

[0033] However, through extensive experiments and analysis, the inventors further discovered that the adhesion of the coating, particularly at the interface between the α-Al₂O₃ layer and the underlying bonding layer, is strongly influenced by the microstructure and crystal orientation of the TiCN layer. The high {211} texture of the TiCN layer promotes the advantages of a highly {001} textured α-Al₂O₃ layer and high flank wear resistance, but it was found that the high {211} texture of the TiCN layer is generally associated with very weak adhesion at the interface between the α-Al₂O₃ and the bonding layer (particularly leading to breakage and chipping at the tool's cutting edge), thereby impairing tool performance and tool life.

[0034] This invention addresses this contradiction through a multilayer wear-resistant hard coating as defined herein, wherein the TiCN layer has a multilayer structure of 5 to 25 alternating C-type and N-type sublayers with well-defined C / N ratios, and wherein the TiCN has a {211} texture represented by a texture factor TC(4 2 2) in a specific range of 3.0 to 5.5. Preferably, the texture factor TC(4 2 2) is 3.5 to 5.5 or 4.0 to 5.3.

[0035] On the one hand, the texture factor TC(4 2 2) of the TiCN layer is sufficiently high to promote the growth and favorable properties of the subsequent α-Al2O3 layer. On the other hand, it has been found that limiting the texture factor TC(4 2 2) of the TiCN layer can reduce or avoid adhesion problems between the α-Al2O3 layer and the bonding layer.

[0036] To achieve these properties, it has been found advantageous to deposit multi-sublayer TiCN layers primarily composed of C-type TiCN, where the growth of C-type TiCN is regularly interrupted by the deposition of N-type TiCN sublayers. It is assumed, and has been found, that the interruption of the C-type TiCN growth conditions by the N-type TiCN sublayers controls the {211} texture of the TiCN layer, denoted herein by the texture factor TC(4 2 2). Given that the C-type TiCN promotes the {211} texture of the TiCN layer, the type and number of N-type TiCN sublayers are suitable for controlling and regulating the constraints of the {211} texture of the TiCN layer. Depositing a single N-type monolayer has also been shown to introduce disadvantages, such as randomly textured crystals and / or very coarse grains.

[0037] It has been shown that optimal properties of the TiCN layer and control of the {211} texture can be achieved if the N-type sublayers in the multi-sublayer structure of the TiCN layer are thinner than the adjacent C-type sublayers. Preferably, each N-type sublayer has a thickness less than 50%, less than 40%, or less than 30% of the thickness of each adjacent C-type sublayer. On the other hand, each N-type sublayer should have a thickness of at least 0.05 μm, at least 0.1 μm, or at least 0.2 μm. Otherwise, the control effect of the N-type sublayers on the texture of the TiCN multilayer would be too low.

[0038] During the deposition of the TiCN layer, the variation between the C-type and N-type sublayers is controlled by changes in deposition conditions, particularly the composition of the reactive gases. The thickness of the C-type and N-type sublayers is controlled by the deposition time under the corresponding C-type and N-type conditions. It should be noted that the deposition rates under different C-type and N-type conditions do not necessarily have to be the same; however, finding the appropriate deposition rate under specific conditions through simple experiments is within the capabilities of those skilled in the art.

[0039] It was also found that, in order to achieve the desired properties of the TiCN layer, the number of alternating C-type and N-type sublayers should not be too low or too high. It has been shown that an alternating number of 5 to 25 C-type and N-type sublayers is advantageous for controlling the {211} texture of the TiCN layer within a favorable texture factor TC (4 2 2).

[0040] According to the present invention, the C-type TiCN sublayer has a C / N ratio in the range of 1.0≤C / N≤2.0, and the N-type TiCN sublayer has a C / N ratio in the range of 0.5≤C / N<1.0. In one embodiment of the present invention, the C-type TiCN sublayer has a C / N ratio in the range of 1.2≤C / N<1.5, and the N-type TiCN sublayer has a C / N ratio in the range of 0.7<C / N<1.0. The effect of interrupting the growth of C-type TiCN by depositing alternating N-type TiCN sublayers is not only influenced by the number of C-type interruptions in the N-type sublayers, but also by the adjustment of the C / N ratio and the difference in C / N ratio between the C-type and N-type sublayers. During the deposition process, the C / N ratio in the deposited layer is adjusted by the deposition conditions, mainly by the ratio of N-donor to C-donor. In a reaction gas system using N₂ and CH₃CN as the N and C sources, the C / N ratio is adjusted by the ratio of these precursor gases.

[0041] According to the present invention, the difference between the C / N ratios of adjacent C-type and N-type layers is ≥0.2. In a preferred embodiment of the present invention, the difference between the C / N ratios of the C-type and N-type layers is in the range of 0.3 to 1.5, or 0.4 to 1.0, or 0.5 to 0.8. If the difference between the C / N ratios of adjacent C-type and N-type layers is too low, the desired effect of controlling the crystalline properties of the TiCN layer is too weak.

[0042] The substrate of the coated cutting tool of the present invention can be any type known in the art that is suitable for metal cutting tools, such as cemented carbide, cermet, ceramics, steel, or cubic boron nitride, with cemented carbide being particularly suitable and preferred.

[0043] It has been demonstrated that the coated cutting tool of the present invention exhibits excellent wear resistance and oxidation resistance as well as enhanced edge toughness in continuous and interrupted cutting, especially in turning operations for ISO P and ISO K steel workpiece applications. Therefore, the present invention includes the use of the coated cutting tool of the present invention for continuous and interrupted cutting of ISO P and ISO K steel materials.

[0044] In a preferred embodiment of the coated cutting tool of the present invention, at least one TiN or TiC base layer is deposited directly on the substrate surface and below the TiCN layer. A suitable base layer has a thickness in the range of 0.3 to 1.5 μm, or 0.3 to 1.0 μm, or 0.3 to 0.7 μm. The base layer can be deposited by thermal HT-CVD or MT-CVD.

[0045] The base layer is adapted to improve the adhesion of the TiCN layer to the substrate. During subsequent high-temperature processing, such as during HT-CVD alumina deposition, the base layer can also serve as a barrier layer to prevent or at least reduce the diffusion of components such as Co from the substrate into the TiCN coating, and vice versa.

[0046] In a preferred embodiment of the coated cutting tool of the present invention, in the multi-sublayer structure of the TiCN layer, the first sublayer above the base layer in the growth direction is a C-type layer. In another preferred embodiment, both the first sublayer above the base layer and the final sublayer below the bonding layer are C-type layers.

[0047] As described above, the main component of the multilayer TiCN layer is C-type TiCN, which has been shown to promote the {211} texture of the TiCN layer. This similarly promotes the {001} texture of the α-Al2O3 layer, and it is preferable to insert the N-type sublayer to control the development of the {211} texture of the TiCN layer. However, if an N-type layer is deposited above the base layer as the first sublayer, it is found that the development of the {211} texture of the TiCN layer is low, resulting in a reduction in the {001} texture of the α-Al2O3 layer. If the final sublayer below the bonding layer is also a C-type layer, the effect may even be enhanced, achieving better control over the {001} texture of the α-Al2O3 layer.

[0048] Regarding the multi-sublayer structure of the TiCN layer, there are two preferred variations of the coated cutting tool of the present invention.

[0049] In a first variant, the first C-type sublayer is relatively thick in the growth direction, having a thickness in the range of 5 to 15 μm, and subsequent C-type sublayers are thinner, having a thickness in the range of 0.5 to 4 μm, wherein a thinner N-type sublayer is deposited between the C-type layers. In this variant, in the first stage, the first thicker C-type sublayer develops a distinct {211} texture and sets a template for subsequent layers.

[0050] In the second variant, each C-type sublayer has a thickness ranging from 0.5 to 4 μm in the growth direction, wherein a thin N-type sublayer is deposited between the C-type layers. This variant also performs well and is particularly suitable if the number of alternating C-type and N-type sublayers in the TiCN layer is within the upper limit and the total thickness of the TiCN layer should not become too high.

[0051] The bonding layer of the coating of the present invention is a monolayer or multilayer oxygen-containing Ti or Ti+Al compound layer deposited above the TiCN layer, having a total thickness of 0.5 μm to 3 μm. Preferably, the bonding layer has a multilayer structure and a total composition of TiCNO or TiAlCNO. During the CVD deposition of the bonding layer, oxygen can be introduced by adding carbon monoxide (CO) to the reactive gas composition. In a preferred embodiment, the deposited bonding layer undergoes an additional oxidation step prior to the subsequent nucleation and growth of the Al2O3 layer. The presence of oxygen in the Ti or Ti+Al bonding layer and the oxidation of the bonding layer surface are suitable for promoting the growth of the Al2O3 layer in α-modification.

[0052] The present invention also includes a method for manufacturing a coated cutting tool as defined herein, wherein the multilayer wear-resistant hard coating is deposited on a substrate by chemical vapor deposition (CVD), the method comprising the following steps:

[0053] - A TiCN layer with a total thickness of 2 μm to 20 μm is deposited by MT-CVD at a reaction temperature in the range of 600 °C to 900 °C using a process gas composition comprising at least TiCl4, H2, N2, and CH3CN, and optionally HCl, in a multi-sublayer structure with a total of p alternating C-type and N-type sublayers, where p is an even or odd number in the range of 5 to 20.

[0054] The C-type and N-type sublayers have different stoichiometry for the atomic ratios of carbon and nitrogen. The C-type TiCN sublayer has a C / N ratio in the range of 1.0 ≤ C / N ≤ 2.0, and the N-type TiCN sublayer has a C / N ratio in the range of 0.5 ≤ C / N < 1.0. The difference between the C / N ratios of adjacent C-type and N-type layers is ≥ 0.2. The C / N ratio is adjusted by the N2 / CH3CN ratio in the process gas composition.

[0055] - By thermal HT-CVD or MT-CVD, a monolayer or multilayer oxygen-containing Ti or Ti+Al compound bonding layer is deposited on top of the TiCN layer with a total thickness of 0.5 μm to 3 μm from a process gas composition containing at least TiCl4, H2, N2, CO, and if Al is present, AlCl3, and optionally CH4 and / or HCl.

[0056] - The bonding layer is oxidized at a temperature in the range of 900-1200°C, a pressure in the range of 30-150 mbar, for a time of 2-20 minutes, and in a gaseous atmosphere containing H2, N2, 1-10 vol% CO2 and 1-20 vol% CO, or a gaseous atmosphere consisting of H2, N2, 1-10 vol% CO2 and 1-20 vol% CO.

[0057] - An α-Al₂O₃ layer with a total thickness of 2 μm to 15 μm is deposited on top of the binding layer treated by the oxidation step via HT-CVD at a reaction temperature in the range of 900 °C to 1200 °C.

[0058] Preferably, the method includes the following further step: depositing at least one TiN or TiC base layer on the substrate surface directly by thermal HT-CVD or MT-CVD using a process gas composition containing at least TiCl4, H2 and N2 to a base layer thickness in the range of 0.3 to 1.5 μm.

[0059] The Ti or Ti+Al compound bonding layer is preferably deposited through multiple subsequent deposition steps to obtain a multi-sublayer structure, wherein each deposition step is performed by HT-CVD at a reaction temperature in the range of 900°C to 1200°C. In the examples herein, the bonding layer is deposited using a five-step process, starting with a TiCN sublayer, followed by several steps under process conditions containing CO in the reaction gas to incorporate oxygen into the layer, and a step containing AlCl3 to incorporate Al into the layer. The overall composition of the bonding layer is Ti+Al+C+N+O. Following the deposition of the bonding layer is an oxidation step at a high temperature of 900°C to 1200°C, preferably about 1000°C, in a gas atmosphere containing H2, N2, CO2, and CO. Attached Figure Description

[0060] Figure 1 Examples of optical micrographs (LOMs) of surfaces polished with a calotte polishing cap are shown. (A) shows coatings of different adhesion grades. Figure 1 a:A = 1; Figure 1 b:A = 2; Figure 1 c:A=3).

[0061] Figure 2 The average values ​​of A-adhesion and Z-adhesion of coated cutting tool samples of the present invention and comparative examples are shown, plotted relative to the number of sublayers in the TiCN layer. Figure 2 a) and the texture factor TC(42 2) relative to the TiCN layer were plotted ( Figure 2 b).

[0062] Figure 3 The cutting time of 12 minutes is shown in the crater wear test (turning operation in C45E steel). Figure 3 a, 3c, 3e) and a cutting time of 15 minutes ( Figure 3 b, 3d, 3f) after the present invention sample ( Figure 3 a, 3b: 4WAG51; Figure 3c, 3d: 4WAG50) and reference sample ( Figure 3 Optical photograph of crescent-shaped crater wear (e, 3f: 1246260).

[0063] Figure 4 It shows Figure 3 The back face wear of samples 4WAG51, 4WAG60 and reference 1246260 shown in the figure after every 3 minutes of cycling in the crescent wear test.

[0064] Figure 5 The flank wear of samples 4WAG51 and 4WAG55 of the present invention and reference sample 1246260 in a toughness test is shown, wherein the maximum wear width is plotted relative to the number of cycles, and the cutting edge damage (ELD) (VB on the flank face) of each sample at the end of tool life is indicated. 最大 ≥0.3mm).

[0065] Figure 6 The TEM image is shown along line AB in the layer growth direction on a sample of the TiCN layer of the present invention. Figure 5 a) and EDXS line scan ( Figure 5 An example of b). In TEM expression, a thicker C-type sublayer (bright) is interrupted by six thin N-type sublayers (dark). EDXS line scans show the atomic percentage concentrations of Ti, C, and N over a length of approximately 4 μm along line AB. In this sample, the average C / N ratio of the C-type sublayers, determined by EDXS, is approximately 1.42, and the average C / N ratio of the N-type sublayers is approximately 0.85. The C / N ratio results can be confirmed by EELS line scans.

[0066] Definitions and methods

[0067] MT-TiCN

[0068] The term “MT-TiCN” as used in this paper means that TICN is deposited by intermediate temperature CVD (MT-CVD), which is different from materials deposited by high temperature CVD (HT-CVD).

[0069] X-ray diffraction (XRD) measurement

[0070] X-ray diffraction measurements were performed on a Panalytical CubiX3 diffractometer using CuKα-radiation and a PIXcel 1D RTMS detector. The X-ray tube was operated with line focusing at 45 kV and 40 mA. Measurements were performed in Bragg-Brentano geometry. On the main beam side, a 0.04 rad Soller slit, a 0.5° fixed divergence slit, and a 1° antiscattering slit were used. A 1.6 mm wide beam mask was inserted to prevent the X-ray beam from overflowing the sample coating. On the secondary beam side, an 8 mm fixed antiscattering slit, a 0.04 rad Soller slit, and a 20 μm thick NiKβ filter were used. Symmetrical θ-2θ scans were performed within an angular range of 19° ≤ 2θ ≤ 130°, with increments of 0.0158° and a counting time of approximately 0.2 seconds.

[0071] Data analysis was performed using a Matlab-based peak fitting procedure by fitting the quasi-Voigt distribution to 2θ scans measured after Cu-Kα2 removal (Rachinger method) and background subtraction. Peak intensities in this paper are peak area intensities. Thin film absorption (TF) corrections were applied to all samples, taking into account the finite thickness of the layer, which is opposite to the natural penetration depth in the bulk material. Furthermore, absorption corrections (Abs) were applied to the layers deposited above the layers of interest. The formulas applied to the TF and Abs corrections are known to those skilled in the art and are as follows:

[0072]

[0073] Specifically, in the case of thin film correction (I TF 校正 In the formula, S is the thickness of the layer of interest, while in the formula used for absorption correction (I0)... Abs 校正 In the formula, S is the thickness of the top absorbing layer. "μ" is the linear absorption coefficient of each layer, where μ(α-Al₂O₃) = 0.01258 μm. -1 And μ(TiCN) = 0.08150 μm -1 (See also: Birkholz, Thin Film Analysis by X-ray Scattering, 2006, Wiley-VCH, ISBN 3-527-31052-5, Chapter 5.5.3, pp. 211-215).

[0074] Because the bonding layer is thinner than the TiCN coating, and has the same crystal structure and similar chemical composition, the overlapping interference peaks of the two layers cannot be separated or reliably deconvoluted. Therefore, instead of performing separate absorption correction and thin film correction on the bonding layer overlapping the TiCN coating, they are treated as a single layer.

[0075] Texture coefficient TC(hkl)

[0076] The term "fiber texture" is often used in conjunction with polycrystalline thin films produced by vapor deposition, describing a preferred crystal orientation of grains grown compared to random orientation, in that a set of geometrically equivalent crystal planes {hkl} are preferably oriented parallel to the substrate surface.

[0077] The preferred growth, i.e., the discovery of a set of geometrically equivalent crystal planes {hkl} preferably parallel to the matrix orientation, is indicated by the texture coefficient TC(hkl) calculated using the formal theory proposed by Harris, based on a defined set of XRD reflections measured on each sample (Harris, GB, Philosophical Magazine Series 7, 43 / 336, 1952, pp. 113-123). According to the Harris formula, the measured peak intensity I(hkl) is related to the relative standard intensity I0(hk1) obtained from the corresponding ICDD PDF card or measured on a standard reference powder.

[0078]

[0079] The texture factor TC(hkl) > 1 for a crystalline material indicates that, at least compared to XRD reflection used in the Harris formula, the grains of the crystalline material are oriented parallel to the matrix surface more frequently than randomly distributed, with respect to their {hkl} crystal planes. For the calculation of the texture factor TC(hkl) in this paper, the measured peak intensity I(hkl) refers to the net peak area intensity corrected as described above.

[0080] For TiCN, ICDD PDF card No. 01-071-6059 was applied, and the following (h kl) reflections (n=7) were used in the calculation:

[0081] {hkl} {1 1 1} {2 0 0} {2 2 0} {3 1 1} {3 3 1} {4 2 0} {4 2 2} <![CDATA[standard intensity I0]]> 803 999 464 198 62 124 100

[0082] For α-Al₂O₃, the standard peak area intensity I₀(hkl) was obtained by measurement on certified NIST (National Institute of Standards and Technology) standard powder SRM676a as described above. The following (hkl) reflection (n=8) was used in the calculation:

[0083] {hkl} {1 0 4} {1 1 0} {1 1 3} {0 2 4} {1 1 6} {3 0 0} {0 0 12} {0 1 14} <![CDATA[Standard intensity I0]]> 87.93 37.68 100.00 45.76 92.43 53.93 2.05 5.16

[0084] Scanning electron microscope (SEM)

[0085] For SEM analysis, the blade was cut into sections, mounted in a holder, and then processed using the following steps: i) grinding with water using a Struers Piano 220 grinding wheel for 6 minutes; ii) polishing with a 9 μm MD-Largo diamond suspension for 3 minutes; iii) polishing with a 3 μm MD-Dac diamond suspension for 3:40 minutes; iv) polishing with a 1 μm MD-Nap diamond suspension for 2 minutes; v) polishing / etching with an OP-S colloidal silica suspension for at least 12 minutes (average particle size of colloidal silica = 0.04 μm). The samples were ultrasonically cleaned prior to SEM examination. SEM images were obtained using a Zeiss Supra 40VP field emission scanning electron microscope with a 30 μm aperture, 2.5 kV accelerating voltage, and a 5 mm working distance.

[0086] Sample preparation for TEM analysis

[0087] Sample preparation for TEM was performed using in-situ extraction techniques, employing a Zeiss Crossbeam 540 field emission scanning electron microscope equipped with a combined FIB / SEM instrument with a gallium liquid metal ion source to cut thin cross-sectional slices from the surface and thin the sample to sufficient electron transparency.

[0088] Analysis of transmission electron microscopy (TEM) studies (STEM-EDXS)

[0089] The imaging was performed using a combination of scanning transmission electron microscopy (STEM) with a primary electron energy of 200 keV and an electron current of 1 nA on the FEI Tecnai Osiris microscope, which is equipped with a high-brightness field emission electron gun and four silicon drift detectors (FEI Super-X EDX system).

[0090] STEM-EDXS mapping was used to determine the sublayer thicknesses of C-type and N-type layers, respectively. The resulting quantitative line profiles of elemental distributions exhibited high uniformity and reproducibility on alternating stacks of C-type and N-type layers. The C / N ratio was determined using line profile fitting in Matlab.

[0091] Electron Energy Loss Spectroscopy (EELS)

[0092] Electron energy loss spectroscopy (EELS) was performed at 300 kV on a FEI Titan 80-300 microscope using a GIF Tridiem 865ER Gatan imaging energy filter. EELS line distribution analysis was performed in STEM mode. High spatial resolution EELS analysis was applied to accurately quantify the C / N ratio. These measurements confirmed the data from the STEM EDXS analysis.

[0093] Cap grinding / Ball crescent cratering

[0094] Cap grinding was used to evaluate coating thickness and adhesion. The blade was placed on a tilted magnetic support of a spherical crescent-shaped grinding device. A spherical cap was ground in the coating and substrate materials by a rotating 30mm steel ball, which was wetted with 3μm water-based struers (DP-Lubricant Green) droplets and driven by a drive shaft at >500 rpm. The grinding process was stopped when the cap diameter in the substrate material reached approximately 600-1100 μm. Taking into account the cap geometry, thickness measurements were performed using an optical microscope (LOM) with dedicated software.

[0095] A-adhesion and Z-adhesion

[0096] “A-adhesion” defines the adhesion between the α-Al2O3 layer and the bonding layer, and “Z-adhesion” defines the internal adhesion within the bonding layer, i.e., between the individual sublayers of the bonding layer. A-adhesion and Z-adhesion are evaluated by observation of LOM on a surface polished with a polishing cap and are visually classified on a scale of 1.0 (= complete adhesion) to 3.0 (= no adhesion).

[0097] The A-adhesion and Z-adhesion criteria at the layer / sublayer interface are as follows:

[0098] A or Z = 1: No breakage or negligible breakage was observed at the interface, and the interface line is intact.

[0099] A or Z=2: Smaller fractures can be observed at the interface, and approximately 51-80% of the total interface line is not deteriorated.

[0100] A or Z=3: Large fractures or continuous delamination can be observed at the interface, with 50-100% of the interface line in the cap deteriorating.

[0101] Figure 1 a, Figure 1 b and Figure 1 c shows an example of A adhesion ( Figure 1 a:A = 1; Figure 1 b:A = 2; Figure 1 c:A=3).

[0102] CVD coating

[0103] All CVD coatings described in this paper were prepared in an industrial-sized Bernex BPX530L radial flow CVD coating chamber with an internal reactor height of 1580 mm, an internal reactor diameter of 500 mm, and an internal volume of approximately 300 liters. Reactive gases were supplied to the reactor through a central gas inlet pipe and introduced into the reaction zone through openings distributed along the inlet pipe to provide a substantially radial gas flow over the substrate.

[0104] It should be noted that a large number of cutting tool substrates (up to approximately 15,000 blades) can be placed in the reactor at different disk levels and at different distances in the radial direction from the reactive gas outlet. Therefore, depending on the total gas flow rate, gas velocity, and type of deposition reaction, the composition of the reactive gas, and consequently the reactivity at different substrate locations within the same reactor, can vary, potentially leading to variations in coating thickness and other product parameters of the coated substrate under the same nominal reaction conditions in the same deposition process. This is a phenomenon well known to those skilled in the art. However, reducing or overcoming such variations to achieve the coating properties of the present invention through adjustments known in the art, such as adjusting the total gas flow rate, gas velocity, deposition time, etc., is within the capabilities of those skilled in the art.

[0105] Unless otherwise specified, in the examples presented herein, the reactor is filled with blades until approximately full capacity, thereby placing the blades of the sample to be studied at three different radial positions (positions: center (C), middle (M), and periphery (P)) on the starting plate from the central inlet pipe and at six different plate levels within the reactor height. The remaining positions on the plates are filled with “waste” blades to approximate full-size deposition conditions and volumes within the reactor as closely as possible.

[0106] Unless otherwise stated, in the examples herein, measurements indicating sample characteristics, such as layer thickness, texture factor, A adhesion and Z adhesion, represent the average values ​​of 18 samples taken from 18 different locations within the reactor, as described above.

[0107] Sandblasting

[0108] If the deposited coating is sandblasted, it is done on the rake face of the cutting tool.

[0109] Dry blasting (“TS”) uses a ZrO2 circular medium with a diameter of 70-120 μm, a blasting pressure of 5 bar (ejector pressure = 1.8 bar), and a blasting distance of 90 mm. Wet blasting (“TT”) uses a blasting slurry (F240 micro-abrasive) of 20% by volume Al2O3 in water, a blasting pressure of 2.8-3.8 bar (ejector pressure = 1.0-2.0 bar), and a blasting distance of 94.5 mm.

[0110] Crescent-shaped pit wear test

[0111] The coated cutting tools were tested in C45E steel using the following cutting data:

[0112] Cutting speed v c 270m / minute

[0113] Cutting feed, f: 0.32 mm / revolution

[0114] Depth of cut, a p 2.5mm

[0115] Blade model: WNMG080412

[0116] (No cutting fluid)

[0117] For each cutting tool, one cutting edge was evaluated. When analyzing crater wear, the area of ​​the exposed substrate was measured using an optical microscope. The tool life was considered reached when the crater wear formed by flowing chips crossed / reached the secondary cutting edge. Wear was evaluated for each cutting tool after 3 minutes of cutting under an optical microscope. Measurements were then taken every 3 minutes of operation, continuing the cutting process until the tool life standard was reached. In addition to crater wear, flank wear was also observed.

[0118] Toughness Test - Edge Line Damage (ELD)

[0119] The coated cutting tools (sandblasted or unsandblasted) were tested during intermittent turning operations on C45E steel using the following cutting data:

[0120] Cutting speed v c 200m / minute

[0121] Cutting feed, f: 0.2mm / revolution

[0122] Depth of cut, a p 2.64mm

[0123] Blade model: WNMG080412

[0124] The workpiece material is C45E. During this type of testing, intermittent cutting processes have proven critical to tool life. If 70% or more of the cutting edge damage (ELD) (Standard #1) or 0.3mm of flank wear (VB) is achieved... 最大 (Standard #2), whichever occurs earlier, is assumed to have reached the end of the tool life. Use a water-miscible metalworking fluid. Example

[0125] matrix

[0126] In this embodiment, a cemented carbide matrix with cutting tool geometry ISO types CNMA120412 and WNMG080412 is used. The cemented carbide composition is 86.11 wt% WC, 5.48 wt% Co, 3.52 wt% TaC, 2.12 wt% TiC, 2.33 wt% NbC, and 0.44 wt% other carbides. The matrix has a Co-rich binder-rich surface region approximately 20 μm from the matrix surface.

[0127] For CVD deposition, two inserts with different geometries, CNMA120412 and WNMG080412, are coated under the same conditions in the same deposition run by placing at least one insert with a CNMA120412 geometry and one insert with a WNMG080412 geometry adjacent to each other in the same radial and disk-level position within the CVD reactor. CNMA120408 inserts are easier to handle due to their simpler geometry and flatter surface. In cutting tests, CNMA120408 inserts are used for coating analysis and measurements (including A-adhesion and Z-adhesion analysis), while WNMG080412 inserts are used for common turning tool insert geometry for steel machining.

[0128] sediment

[0129] The coating sequence in the embodiments described herein is: TiN base layer / TiCN coating (MT-TiCN) / TiAlCNO bonding layer / α-Al2O3 layer. An oxidation step is applied to the bonding layer prior to the deposition of the α-Al2O3 layer. In all embodiments and comparative examples of the invention prepared herein, the TiN base layer, the TiAlCNO bonding layer, the oxidation step, and the α-Al2O3 layer were deposited and performed under the same process conditions to ensure comparability of the embodiments relative to variations of single-layer or multi-layer TiCN coatings.

[0130] Table 1 shows the process parameters used to deposit the layers of the samples of the present invention and the comparative samples, and Table 3 shows the TiCN coating sequence. Table 2 shows the process steps and parameters used to deposit the layer of reference sample 1246260. Table 4 shows the parameters measured on the samples (averages of 18 samples of the present invention and the comparative samples distributed in the reactor, as described above).

[0131] The TiN base layer is approximately 0.3-0.5 μm thick. The TiAlCNO bonding layer is approximately 1.0-1.5 μm thick. The α-Al₂O₃ layer is approximately 5.5-6.5 μm thick. The TiCN coating is approximately 7.5-11.0 μm thick.

[0132] The bonding layer consists of a multilayer structure deposited in five coating steps BL-a to Be. The deposition of α-Al2O3 is carried out in two steps, namely step 1 and step 2.

[0133] Adhesion analysis

[0134] The average values ​​of A-adhesion and Z-adhesion of the sample of the present invention and the comparative sample were measured respectively (see Tables 3 and 4), and relative to the number of multilayers ( Figure 2 a; #-ML) and the texture coefficient TC(4 2 2)( of the TiCN layer) Figure 2 b) Drawing. In Figure 2 a and Figure 2 The dashed box in b indicates the monolayer samples (#-ML = 1) using TiCN-C and TiCN-D. The results show that even for these monolayer samples, #-ML and TC(4 2 2) have almost no effect on Z-adhesion. However, a strong negative linear dependence of A-adhesion relative to #-ML and a strong positive linear dependence of A-adhesion relative to TC(4 2 2) were observed. Both monolayer examples exhibited very weak A-adhesion. Multilayer samples within the TC(4 2 2) range of the #-ML and TiCN layers of the present invention exhibited improved A-adhesion, along with improved cutting performance.

[0135]

[0136]

[0137]

[0138] Table 3: TiCN coating sequences in the present invention sample and comparative samples

[0139]

[0140] Toughness test

[0141] Cutting edge toughness tests were performed on the reference sample (1246260) and two samples of the present invention (4WAG51 and 4WAG55). As described above, each sample underwent post-treatment, “TS+TT” = dry blasting followed by wet blasting. All samples reached or exceeded 0.3 mm of flank wear VB well before reaching 70% cutting edge damage (ELD) (tool life end criterion #1). 最大 (Tool life termination criterion #2). Therefore, ELD was determined for each sample after tool life termination due to flank wear. The results are shown in Table 5 below. Figure 5 As shown in the image.

[0142] Table 5: Cutting edge toughness test

[0143]

[0144] Crescent-shaped pit wear

[0145] As described above, the crater wear tests of the present invention samples 4WAG51 and 4WAG60 and the reference sample 1246260 were performed for 12 minutes and 15 minutes respectively (the turning operation was carried out in C45E steel). Figure 3 The observed (LOM) wear of the sample of the present invention is shown. Figure 3 a = 4WAG51, 12 minutes; Figure 3 b = 4WAG51, 15 minutes Figure 3 c = 4WAG60, 12 minutes; Figure 3 d = 4WAG60, 15 minutes; Figure 3 e = 1246260, 12 minutes; Figure 3 (f = 1246260, 15 minutes). The results showed that the crater wear of the present invention sample and the reference sample was similar after 12 minutes, but after 15 minutes, the wear of the present invention sample was still acceptable, while the cutting edge, rake face, and flank face of the reference sample were almost completely destroyed. Figure 4 The wear on the back face of the sample is shown after every 3 minutes of cycling in the crescent wear test.

Claims

1. A coated cutting tool for chip-forming metalworking, comprising a substrate and a multilayer wear-resistant hard coating, said multilayer wear-resistant hard coating comprising: a) A TiCN layer having a total thickness of 2 µm to 20 µm. The TiCN layer has a multi-sublayer structure with a total of p alternating C-type and N-type sublayers, where p is an even or odd number in the range of 5 to 25. In the multi-sublayer structure of the TiCN layer, the thickness of each N-type sublayer is less than 50% of that of each adjacent C-type sublayer. The C-type and N-type sublayers have different stoichiometry for the atomic ratios of carbon and nitrogen, wherein the C-type TiCN sublayer has a C / N ratio in the range of 1.0 ≤ C / N ≤ 2.0, and the N-type TiCN sublayer has a C / N ratio in the range of 0.5 ≤ C / N < 1.0, and wherein the difference between the C / N ratios of adjacent C-type and N-type layers is ≥ 0.

2. The TiCN layer therein has an overall fiber texture characterized by a texture factor TC(4 2 2) in the range of 3.0 to 5.5, wherein TC(4 2 2) is defined as follows: in I(hkl) =(hkl) XRD intensity of reflection I 0 (hkl) =Standard intensity based on standard powder diffraction data from ICDD PDF card No. 01-071-6059 n=7 = the number of reflections used in the calculation, of which the seven (hkl) reflections used are: (1 1 1), (2 0 0), (22 0), (3 1 1), (3 3 1), (4 2 0) and (4 2 2). b) A single-layer or multi-layer oxygen-containing Ti or Ti+Al compound bonding layer, said bonding layer having a total thickness of 0.5 µm to 3 µm above the TiCN layer. c) An α-Al₂O₃ layer, located above the bonding layer, having a total thickness of 2 µm to 15 µm. The α-Al₂O₃ layer has an overall fibrous texture characterized by a texture factor TC(0 0 12) > 5, where TC(0 0 12) is defined as follows: in I(hkl) =(hkl) XRD intensity of reflection I 0 (hkl) Standard strength measured on NIST standard powder SRM676a n = 8 = the number of reflections used in the calculation, where the eight (hkl) reflections used are: (1 0 4), (1 1 0), (1 1 3), (0 2 4), (1 1 6), (3 0 0), (0 0 12), and (0 1 14). The standard strength has the following values:

2. The coated cutting tool according to claim 1, wherein at least one TiN or TiC base layer is deposited directly on the surface of the substrate and below the TiCN layer, the base layer having a thickness in the range of 0.3 to 1.5 µm, 0.3 to 1.0 µm, or 0.3 to 0.7 µm.

3. The coated cutting tool according to claim 1 or 2, wherein the TiCN layer has an overall fibrous texture characterized by a texture factor TC(42 2) in the range of 3.5 to 5.5 or 4.0 to 5.

3.

4. The coated cutting tool according to claim 1 or 2, wherein in the multi-sublayer structure of the TiCN layer, the first sublayer above the base layer and the final sublayer below the bonding layer are C-type layers in the growth direction.

5. The coated cutting tool according to claim 1 or 2, wherein in the multi-sublayer structure of the TiCN layer, the thickness of each N-type sublayer is less than 40% or less than 30% of that of each adjacent C-type sublayer.

6. The coated cutting tool according to claim 1 or 2, wherein, In the multi-sublayer structure of the TiCN layer, each N-type sublayer has a thickness of at least 0.05 µm, at least 0.1 µm, or at least 0.2 µm.

7. The coated cutting tool according to claim 1 or 2, wherein in the multi-sublayer structure of the TiCN layer, in the growth direction - The first C-type sublayer has a thickness ranging from 2 to 15 µm, and subsequent C-type sublayers have a thickness ranging from 0.5 to 4 µm, or - All C-type sublayers have a thickness ranging from 0.5 to 4 µm.

8. The coated cutting tool according to claim 1 or 2, wherein the Ti or Ti+Al compound bonding layer has a multi-sublayer structure and has a total composition of TiCNO or TiAlCNO.

9. The coated cutting tool according to claim 1 or 2, wherein the substrate is composed of cemented carbide, cermet, ceramic, steel, or cubic boron nitride.

10. The coated cutting tool according to claim 1 or 2, wherein the hard coating layer is deposited by chemical vapor deposition (CVD), the TiCN is an MT-TiCN layer deposited by MT-CVD at a reaction temperature in the range of 600°C to 900°C, and / or the Ti or Ti+Al compound bonding layer is deposited by HT-CVD at a reaction temperature in the range of 900°C to 1200°C, and / or the α-Al2O3 layer is deposited by HT-CVD at a reaction temperature in the range of 900°C to 1200°C.

11. Use of the coated cutting tool according to any one of claims 1 to 10 for continuous and intermittent chip-forming machining of ISO P or ISO K steel materials.

12. Use of the coated cutting tool according to any one of claims 1 to 10 for turning operations of ISO P or ISO K steel materials.

13. A method for manufacturing a coated cutting tool as defined in any one of claims 1 to 10, wherein the multilayer wear-resistant hard coating is deposited on the substrate by chemical vapor deposition (CVD), the method comprising the steps of: - A TiCN layer is deposited to a total thickness of 2 µm to 20 µm by MT-CVD at a reaction temperature in the range of 600 °C to 900 °C using a process gas composition containing at least TiCl4, H2, N2, and CH3CN, or a process gas composition containing at least TiCl4, H2, N2, CH3CN, and HCl, in a multi-sublayer structure with a total of p alternating C-type and N-type sublayers, where p is an even or odd number in the range of 5 to 20. In the multi-sublayer structure of the TiCN layer, the thickness of each N-type sublayer is less than 50% of that of each adjacent C-type sublayer. The C-type and N-type sublayers have different stoichiometry for the atomic ratios of carbon and nitrogen. The C-type TiCN sublayer has a C / N ratio in the range of 1.0 ≤ C / N ≤ 2.0, and the N-type TiCN sublayer has a C / N ratio in the range of 0.5 ≤ C / N < 1.

0. The difference between the C / N ratios of adjacent C-type and N-type layers is ≥ 0.

2. The C / N ratio is adjusted by the N2 / CH3CN ratio in the process gas composition. - By thermal HT-CVD or MT-CVD, an oxygen-containing Ti compound bonding layer of monolayer or multilayer is deposited on top of the TiCN layer with a total thickness of 0.5 µm to 3 µm using a process gas composition containing at least TiCl4, H2, N2, and CO. A monolayer or multilayer oxygen-containing Ti compound bonding layer with a total thickness of 0.5 µm to 3 µm is deposited over the TiCN layer by thermal HT-CVD or MT-CVD using a process gas composition containing at least TiCl4, H2, N2, and CO, and CH4 and / or HCl. A monolayer or multilayer oxygen-containing Ti+Al compound bonding layer with a total thickness of 0.5 µm to 3 µm is deposited over the TiCN layer by thermal HT-CVD or MT-CVD using a process gas composition containing at least TiCl4, H2, N2, CO, and AlCl3. An oxygen-containing Ti+Al compound bonding layer, consisting of a monolayer or multilayer, is deposited on top of the TiCN layer using thermal HT-CVD or MT-CVD with a process gas composition comprising at least TiCl4, H2, N2, CO, and AlCl3, as well as CH4 and / or HCl, to a total thickness of 0.5 µm to 3 µm. - The bonding layer is oxidized at a temperature ranging from 900 to 1200°C, a pressure ranging from 30 to 150 mbar, for a time of 2 to 20 minutes, in a gaseous atmosphere containing H2, N2, 1-10 vol% CO2, and 1-20 vol% CO (composed of H2, N2, 1-10 vol% CO2, and 1-20 vol% CO). - An α-Al₂O₃ layer with a total thickness of 2 µm to 15 µm is deposited on top of the binding layer treated by the oxidation step via HT-CVD at a reaction temperature in the range of 900 °C to 1200 °C.

14. The method of claim 13, comprising the step of: depositing at least one TiN or TiC base layer to a base layer thickness in the range of 0.3 to 1.5 µm directly on the surface of the substrate by thermal HT-CVD or MT-CVD using a process gas composition containing at least TiCl4, H2 and N2.

15. The method according to claim 13 or 14, wherein the Ti or Ti+Al compound binding layer is deposited by a plurality of subsequent deposition steps to obtain a multilayer structure, wherein each deposition step is performed by HT-CVD at a reaction temperature in the range of 900°C to 1200°C.

Citation Information

Patent Citations

  • Surface-coated member

    US7172807B2

  • Coated cutting tool

    CN110268081A

  • Metal cutting tool with multi-layer coating

    US20200181756A1