Single-phase nd-fe-pd alloy magnetic refrigeration material based on rapid annealing process and preparation method thereof
Single-phase Nd₆Fe₁₃Pd magnetic refrigeration materials were prepared by a combination of strip spinning and rapid annealing processes. This solved the problem of poor magnetic entropy change performance caused by excessively long or short annealing times in existing technologies, and achieved efficient preparation and excellent magnetic refrigeration performance.
Patent Information
- Application Number
- CN202311583206.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-24
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-11-24
AI Technical Summary
In the preparation of single-phase Nd₆Fe₁₃Pd magnetic refrigeration materials, existing technologies cannot obtain a single-phase structure when the annealing time is too long or too short, resulting in poor magnetic entropy change performance.
By employing strip spinning technology and rapid annealing process, single-phase Nd₆Fe₁₃Pd alloy is prepared by preparing Nd-Fe-Pd alloy ingots into thin strips, annealing them at 823K for 5 minutes, and then rapidly cooling them.
A single-phase Nd₆Fe₁₃Pd alloy was obtained in a short time, with a magnetic entropy change of 3.4 J kg⁻¹K⁻¹ and a cooling capacity of 220 J/kg, which significantly improved the cooling performance.
Smart Images

Figure CN117583564B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of magnetic refrigeration, specifically to a single-phase Nd-Fe-Pd alloy magnetic refrigeration material based on a rapid annealing process and its preparation method. Background Technology
[0002] Nd6Fe 13 Pd is a low-melting-point alloy without heavy rare earth elements, which can lower the heat treatment temperature of NdFeB magnets and significantly improve the microstructure of magnet grain boundaries during tempering. It can diffuse rapidly within NdFeB magnets, which is beneficial for improving the wettability of the liquid phase along the main phase particles. Meanwhile, Nd6Fe... 13 Pd can also alter the physicochemical properties of intercrystalline phases, further enhancing the intrinsic coercivity, maximum energy product, and thermal stability of magnets. Currently, the preparation of single-phase Nd6Fe... 13 Pd magnetic refrigeration materials are annealed using conventional methods. Conventional annealing involves slowly heating the metal to a certain temperature, holding it for a sufficient time to allow changes in the metal's internal crystal structure, and then cooling it at a suitable rate, maintaining the crystal structure in its new state. This is often referred to as direct ingot annealing. However, conventional annealing methods generally suffer from the problem of long annealing times.
[0003] For example, existing literature 1 (K. Niitsu, R. Kainuma. Phase equilibria in the Fe-La-Siternary system[J], Intermetallics, 2012, 20: 160-169.) uses La(Fe,Si) 13 La(Fe,Si) was prepared by annealing the ingot at 1323 K for 7-14 days. 13 Magnetic refrigeration materials. This literature demonstrates the following principle: with increasing annealing time, La(Fe,Si)... 13 The more homogeneous the phase, the lower the proportion of the α-(Fe,Si) phase. After annealing for 14 days, a single-phase La(Fe,Si) phase is obtained. 13 The technical effects of magnetic refrigeration materials.
[0004] For example, existing literature 2 (S. Fujieda, K. Fukamichi, S. Suzuki. Microstructure and isothermal magnetic entropy change of La(Fe) 0.89 Si0 .11 ) 13in a single-phaseformation process by annealing[J],Journal of Alloys and Compounds,2013,566:196-200.) by converting La(Fe 0.89 Si0 .11 ) 13 Single-phase La(Fe) was prepared by annealing the ingot at 1323K for 300 hours. 0.89 Si0 .11 ) 13 A magnetic refrigeration material was obtained, yielding a magnetic entropy change of 24 J / kg. -1 K -1 The technical effect.
[0005] As can be seen from existing literature 1 and literature 2, the above technical solutions all employ conventional annealing methods. Although they all yield single-phase magnetic refrigeration materials, the annealing time requires at least 7-14 days. Reducing the annealing time is a technical problem that needs to be solved by conventional annealing methods.
[0006] For example, existing literature 3 (J.Yang, Y.Shao, MX.Zhang, YF.Liu, A.Yan, J.Liu. The influence of Ce on microstructure, phase formation and magnetocaloric properties in off-stoichiometric La 2-x Ce x Fe 11 Si2 alloys[J], Intermetallics, 2018, 103: 97-100) by (La,Ce)1(Fe,Si) 13 (La,Ce)1(Fe,Si) was prepared by annealing the ingot at 1423K for 12 hours. 13 A magnetic refrigeration material was developed, achieving a magnetic entropy change of 21.8 J / kg. -1 K -1 The technical effect; in particular, the obtained material contains not only (La,Ce)(Fe,Si) 13 The phases also include La5Si3 and (La,Ce)2(Fe,Si). 17 LaFeSi and α-Fe phases.
[0007] A comparison of existing literature 3 and existing literature 2 shows that shortening the annealing time leads to (La,Ce)1(Fe,Si) 13The presence of multiple phases prevents the formation of a single-phase magnetic refrigeration material, resulting in a decrease in magnetic entropy change performance from 24 J / kg. -1 K -1 Reduced to 21.8 J kg -1 K -1 .
[0008] Based on the above, regarding La(Fe,Si) 13 An analysis of relevant literature on magnetic refrigeration materials leads to the following conclusions:
[0009] 1. Single-phase La(Fe,Si) can be obtained through conventional annealing methods. 13 It is a magnetic refrigeration material, and it has good magnetic entropy change performance;
[0010] 2. Directly reducing the annealing time cannot yield single-phase La(Fe,Si). 13 Magnetic cooling materials, which leads to a decrease in magnetic entropy change performance.
[0011] Therefore, some studies use strip spinning technology instead of conventional annealing methods to prepare magnetic refrigeration materials. Strip spinning technology rapidly cools the alloy to obtain amorphous to microcrystalline thin strips, which are then heat-treated to obtain the magnetic refrigeration material; this is simply referred to as strip spinning followed by annealing.
[0012] For example, existing literature 4 (XLH,Y.Tian,Y.Xue,C Liu,W.Xia,H.Xu,PL Kelley,H.Srikanth,MHPhan.Formation of tree-like and vortex magnetic domains of nanocrystalline α-(Fe,Si)in La-Fe-Si ribbons during rapid solidification and subsequent annealing[J].Journal of Alloys and Compounds,2016,669:205-209.) first obtains La(Fe,Si) at a ribbon spinning speed of 35 m / s. 13 The alloy strip, after being annealed at 1273K for 2 hours, yields a uniform single-phase La(Fe,Si). 13 Magnetic refrigeration materials. The principle of this technical solution is to crystallize the amorphous phase into La(Fe,Si) through annealing. 13 Simultaneously, a peritectic reaction occurs. La(Fe,Si) is generated. 13Based on the above principle, when obtaining a single-phase structure by first using a strip-spinning technique followed by annealing, the annealing time can be significantly reduced. It should be noted that the annealing time still needs to be 2 hours. Furthermore, this literature provides an experiment with annealing for 3 minutes under the same conditions. Experimental results show that La(Fe,Si)... 13 In addition to the main phase La(Fe,Si), the alloy ribbon also contains... 13 In addition, there are also impurity phases α-(Fe,Si) and LaFeSi. In other words, this literature proves that even with the strip spinning technique, an excessively short annealing time cannot achieve the technical effect of a single-phase alloy.
[0013] To summarize the conclusions of the above literature, we can draw the following two points:
[0014] 1. The conventional annealing method based on ingot casting is used to obtain single crystal structures, and the required annealing time is calculated in weeks;
[0015] 2. The annealing method based on the strip spinning technique to obtain a single crystal structure still requires time calculated in hours.
[0016] The above La(Fe,Si) 13 The technical problems and related conclusions faced by the alloy, and the Nd6Fe involved in this invention. 13 Pd magnetic refrigeration materials also face similar technical challenges.
[0017] For example, existing literature 5 (YSDu.CHZhang,YM Lu,L.Li,JQLi,L.Ma,GHRao. Table-like magnetocaloric effect and large refrigerant capacity in Nd6Fe) 13 Pd 1-x Ag x compounds[J].
[0018] Intermetallics, 2021, 130:107062.) also uses conventional annealing methods to prepare single-phase Nd6Fe. 13 Pd, specifically, by using Nd6Fe 13 Single-phase Nd₂Fe was prepared by annealing Pd ingots at 823K for 30 days. 17 A magnetic refrigeration material was obtained, achieving a magnetic entropy change of 3.4 J / kg. -1 K -1 The technical effect.
[0019] However, the inventors of this invention performed an annealing treatment of Nd6Fe based on the strip spinning technique. 13When working with Pd alloys, it was found that under conditions similar to La(Fe,Si), at 823K, [the following conditions were observed]. 13 The annealing time of the alloy cannot produce single-phase Nd6Fe. 13 Based on fundamental knowledge in alloy heat treatment, extending the annealing time will not yield single-phase Nd6Fe. 13 Therefore, the technical problem to be solved by this invention is how to prepare Nd6Fe with a single-phase structure under annealing conditions based on the strip spinning technique. 13 Pd alloy. Summary of the Invention
[0020] The purpose of this invention is to provide a single-phase Nd-Fe-Pd alloy magnetic refrigeration material based on a rapid annealing process and its preparation method. Through strip spinning technology and annealing conditions, Nd6Fe with a single-phase structure is prepared. 13 Pd alloy.
[0021] To achieve the above-mentioned objectives, the technical solution adopted by this invention is as follows:
[0022] A single-phase Nd-Fe-Pd alloy magnetic refrigeration material based on a rapid annealing process is obtained by spinning an Nd-Fe-Pd alloy ingot to obtain an Nd-Fe-Pd alloy strip, followed by rapid annealing to obtain the Nd-Fe-Pd magnetic refrigeration material; the composition of the Nd-Fe-Pd magnetic refrigeration material is single-phase Nd6Fe. 13 Pd has a tetragonal crystal structure and its space group is I4 / mcm.
[0023] A method for preparing a single-phase Nd-Fe-Pd alloy magnetic refrigeration material based on a rapid annealing process includes the following steps:
[0024] Step 1, smelting of Nd-Fe-Pd alloy ingots: First, according to the chemical formula Nd6Fe... 13 Pd, Nd, Fe, and Pd are weighed as raw materials, first cleaned with high-purity argon gas, then smelted under certain conditions by tumbling, and finally cooled to room temperature in the furnace to obtain Nd6Fe. 13 Pd alloy ingots, abbreviated as Nd-Fe-Pd alloy ingots;
[0025] In step 1, the amount of Nd added needs to be increased by 2 wt.% on top of the theoretical content as compensation for loss;
[0026] The cleaning conditions are as follows: a vacuum degree ≤ 2 × 10⁻⁶. -3 Under the condition of Pa, clean with high-purity argon gas 2-3 times;
[0027] The conditions for the inverted melting are: the protective gas is high-purity argon, the gas pressure is 1 bar, and the number of melting cycles is 3.
[0028] Step 2, preparation of Nd-Fe-Pd alloy thin strips: First, the Nd-Fe-Pd alloy ingot obtained in Step 1 is heated to a liquid state. Then, it is vacuum-spinned under certain conditions to obtain Nd6Fe. 13 Pd alloy thin strips are simply referred to as Nd-Fe-Pd alloy thin strips;
[0029] In step 2, the vacuum belt spinning condition is that the spinning speed is 30m / s;
[0030] Step 3: Annealing of Nd-Fe-Pd alloy strips. Under certain conditions, the Nd-Fe-Pd alloy strips obtained in Step 2 are annealed to obtain Nd6Fe. 13 Pd alloy magnetic refrigeration materials, or simply Nd-Fe-Pd magnetic refrigeration materials.
[0031] In step 3, the annealing conditions are: annealing temperature of 823K, annealing time of 5min, and immediately after annealing, the Nd-Fe-Pd alloy strip is placed in an ice-water mixture to be rapidly cooled to room temperature.
[0032] An application of a single-phase Nd-Fe-Pd alloy magnetic refrigeration material based on a rapid annealing process is presented. The Nd-Fe-Pd magnetic refrigeration material has a transition temperature of 163 K, and an antiferromagnetic to ferromagnetic transition occurs with decreasing temperature, followed by a first-order magnetic phase transition near the transition temperature. Under a magnetic field of 0-5 T, the magnetization measured at 125 K is 139 emu / g, and the maximum magnetic entropy change is 3.4 J kg. -1 K -1 Its cooling capacity reaches 220J / kg.
[0033] The performance of this invention can be seen from the following tests.
[0034] XRD and EM tests confirmed that the Nd-Fe-Pd magnetic refrigeration material is Nd6Fe. 13 Nd6Fe, a single-phase compound with a Si-type tetragonal structure. 13 Pd, with space group I4 / mcm. The Nd-Fe-Pd magnetic refrigeration material has a uniform phase composition of Nd6Fe. 13 Pd single-phase compound.
[0035] Thermomagnetic FC curve tests under field cooling conditions show that the transition temperature of the Nd-Fe-Pd magnetic refrigeration material is 163K, and an antiferromagnetic-ferromagnetic transition occurs as the temperature decreases.
[0036] Isothermal magnetization tests revealed that, in the 0-5T magnetic field near the transition temperature, the magnetization curves below the transition temperature showed that the sample was rapidly magnetized and tended to saturate with only a small magnetic field, exhibiting obvious ferromagnetic characteristics. Above the transition temperature, the magnetization curves showed a linear increase under relatively low magnetic fields. When the magnetic field increased to a certain magnitude, the magnetization intensity increased rapidly, showing a distinct "inflection point," indicating an antiferromagnetic to ferromagnetic phase transition. The magnetization intensity measured at 125K was 139 emu / g.
[0037] M was obtained by isothermal magnetization curve 2 Arrott curves obtained through -H / M treatment show that the slope of the curve becomes negative near the transformation temperature, exhibiting an S-shaped curve. This indicates that a first-order magnetic phase transition occurs in this type of alloy near the transformation temperature. Therefore, the Nd-Fe-Pd magnetic refrigeration material undergoes a first-order magnetic phase transition near the transformation temperature.
[0038] Magnetothermic performance tests show that the maximum magnetic entropy change of the Nd-Fe-Pd magnetic refrigeration material under a magnetic field of 0-5T is 3.4 J / kg. -1 K -1 The maximum cooling capacity is 220J / kg.
[0039] Therefore, based on the above tests, this invention has the following advantages over the prior art: By adjusting the annealing time and the spinning speed, this invention can obtain a single-phase Nd-Fe-Pd magnetic refrigeration material with a maximum magnetic entropy change of 3.4 J kg at annealing at 823 K for 5 minutes. -1 K -1 The technical effect is a maximum cooling capacity of 220 J / kg. Specifically, compared with existing literature 5 in the background art, the present invention and existing literature 5 also obtain single-phase Nd-Fe-Pd magnetic refrigeration materials, and the magnetic entropy change reaches 3.4 J / kg. -1 K -1 Under the premise that the existing literature 5 requires an annealing time of 30 days, the present invention only requires 5 minutes. Attached image description:
[0040] Figure 1 The XRD pattern of the Nd-Fe-Pd alloy thin strip obtained in step 2 of Example 1;
[0041] Figure 2 This is a SEM image of the Nd-Fe-Pd alloy thin strip obtained in step 2 of Example 1;
[0042] Figure 3 The XRD pattern of the Nd-Fe-Pd magnetic refrigeration material of Example 1 at room temperature.
[0043] Figure 4 The image shows a SEM image of the Nd-Fe-Pd magnetic refrigeration material from Example 1.
[0044] Figure 5 The thermomagnetic curve of the Nd-Fe-Pd magnetic refrigeration material in Example 1 under an external magnetic field of 200 Oe is shown.
[0045] Figure 6 The isothermal magnetization curve of the Nd-Fe-Pd magnetic refrigeration material in Example 1 near the transition temperature;
[0046] Figure 7 The Arrott curve of the Nd-Fe-Pd magnetic refrigeration material in Example 1 near the transition temperature;
[0047] Figure 8 The isothermal magnetic entropy change curves of the Nd-Fe-Pd magnetic refrigeration material in Example 1 under a varying magnetic field of 0-5T.
[0048] Figure 9 The XRD pattern of Nd-Fe-Pd-2h at room temperature is shown in Comparative Example 1.
[0049] Figure 10 The XRD pattern of Nd-Fe-Pd-4h at room temperature is shown in Comparative Example 2.
[0050] Figure 11 The XRD pattern of Nd-Fe-Pd-8D at room temperature is shown in Comparative Example 3.
[0051] Figure 12 The XRD pattern of Nd-Fe-Pd-25 at room temperature is shown in Comparative Example 4.
[0052] Figure 13 The image shows the XRD pattern of Nd-Fe-Pd-35 at room temperature for Comparative Example 5. Detailed Implementation
[0053] The present invention will be further described in detail through embodiments and with reference to the accompanying drawings, but this is not intended to limit the scope of the invention.
[0054] Example 1
[0055] A method for preparing single-phase Nd-Fe-Pd alloy magnetic refrigeration material based on rapid annealing process, the specific steps of which are as follows:
[0056] Step 1, smelting of Nd-Fe-Pd alloy ingots: First, according to the chemical formula Nd6Fe... 13 Pd, Nd, Fe and Pd are weighed as raw materials, with the amount of Nd added 2 wt.% above the theoretical content as compensation for loss. Then, under a vacuum of 2×10 -3Under the condition of Pa, after purging twice with high-purity argon, the furnace is tumbled and melted at 1 bar of high-purity argon for 3 times. After melting, the furnace is cooled to room temperature to obtain Nd6Fe. 13 Pd alloy ingots, abbreviated as Nd-Fe-Pd alloy ingots;
[0057] Step 2, Preparation of Nd-Fe-Pd alloy thin strip: First, the Nd-Fe-Pd alloy ingot obtained in Step 1 is heated to a liquid state. Then, it is vacuum-spun at a spinning speed of 30 m / s to obtain Nd6Fe 13 Pd alloy thin strips are simply referred to as Nd-Fe-Pd alloy thin strips;
[0058] Step 3: Annealing of Nd-Fe-Pd alloy strip. The annealing temperature is 823K and the annealing time is 5min. After annealing, the Nd-Fe-Pd alloy strip is immediately placed in an ice-water mixture to be rapidly cooled to room temperature. The Nd-Fe-Pd alloy strip obtained in Step 2 is then subjected to annealing treatment to obtain a single-phase Nd-Fe-Pd alloy magnetic refrigeration material based on rapid annealing process and its preparation method, which is referred to as Nd-Fe-Pd magnetic refrigeration material.
[0059] To verify the crystal structure and phase composition of the Nd-Fe-Pd magnetic refrigeration material, XRD and SEM tests were performed. Meanwhile, to further confirm the effect of the annealing treatment in step 3 on the crystal structure and phase composition of the material, XRD and SEM tests were performed on the Nd-Fe-Pd alloy thin strip obtained in step 2.
[0060] The XRD test results of the Nd-Fe-Pd alloy thin strip are as follows: Figure 1 As shown, the main phase of the obtained Nd-Fe-Pd alloy ribbon is Nd2Fe. 17 There is still an uncrystalline phase present; SEM test results are as follows: Figure 2 As shown, the results indicate that the main phase of the Nd-Fe-Pd alloy ribbon sample is Nd2Fe. 17 The rest are amorphous phases.
[0061] The XRD test results of Nd-Fe-Pd magnetic refrigeration materials are as follows: Figure 3 As shown, the results indicate that the Nd-Fe-Pd magnetic refrigeration material is Nd6Fe 13 Nd6Fe, a single-phase compound with a Si-type tetragonal structure. 13 Pd, its space group is I4 / mcm; SEM test results are as follows Figure 4 As shown, the Nd-Fe-Pd magnetic refrigeration material has a uniform phase composition of Nd6Fe. 13 Pd single-phase compound.
[0062] The XRD and SEM test results above show that the annealing treatment in step 3 can achieve the conversion of Nd2Fe into Nd2Fe. 17 Phase transformation to Nd6Fe 13 Pd phase. The principle is that Nd6Fe... 13 The solidification process of Pd compounds is as follows: the coarse crystalline phase Fe first solidifies from the liquid phase and precipitates L→Fe, and a eutectic reaction occurs as the temperature decreases. What happened next The peritectic reaction produces the ternary compound Nd6Fe. 13 Therefore, annealing Nd-Fe-Pd alloy strips can achieve Nd2Fe 17 Peritectic reaction produces Nd6Fe 13 Pd.
[0063] To demonstrate that the Nd-Fe-Pd magnetic refrigeration material exhibits magnetic transition characteristics under low field conditions, thermomagnetic FC curve tests were conducted under field-cooled conditions. The test results are as follows: Figure 5 As shown, only one magnetic transition occurred within the test temperature range of 10-300K, and an antiferromagnetic-ferromagnetic transition occurred as the temperature decreased; further as... Figure 5 As shown in the inset, the transition temperature is defined as 163K by the dM / dT-T curve, that is, the transition temperature of the Nd-Fe-Pd magnetic refrigeration material is 163K.
[0064] To demonstrate the isothermal magnetization behavior of the Nd-Fe-Pd magnetic refrigeration material, isothermal magnetization tests were conducted at magnetic fields ranging from 0 to 5 T and from 125 to 253 K near the transition temperature. The test results are as follows: Figure 6 As shown, the magnetization intensity measured at 125 K was 139 emu / g. The test results indicate that below the transition temperature, the magnetization curve shows that the sample is rapidly magnetized to saturation with only a small magnetic field, exhibiting obvious ferromagnetic characteristics. Above the transition temperature, the magnetization curve shows a linear increase under relatively low magnetic fields. When the magnetic field increases to a certain magnitude, the magnetization intensity increases rapidly, showing a clear "inflection point," indicating an antiferromagnetic to ferromagnetic phase transition.
[0065] To further demonstrate the magnetic transition type of the Nd-Fe-Pd magnetic refrigeration material, the isothermal magnetization curves were subjected to M-wave analysis. 2 Arrott curves were obtained through -H / M processing. The processing results are as follows: Figure 7As shown, the Arrott curves exhibit negative slopes and S-shaped curves near the transition temperature. Based on the results from reference 1 (SK Banerjee. On a generalized approach to first and second order magnetic transitions[J]. Physics Letters 1964, 12:16.), the Arrott curves for first-order phase change materials near the phase transition temperature show negative slopes or inflection points, while the Arrott curves for second-order phase change materials show positive slopes near the phase transition temperature. This indicates that the Nd-Fe-Pd magnetic refrigeration material undergoes a first-order magnetic phase transition near the transition temperature.
[0066] To demonstrate the magnetocaloric properties of Nd-Fe-Pd magnetic refrigeration materials, according to Equation 1, Maxwell's equations:
[0067]
[0068] The magnetic entropy change was obtained by calculating the isothermal magnetization curve. The calculation results are as follows: Figure 8 As shown, under a varying magnetic field of 5T, the maximum magnetic entropy change of the Nd-Fe-Pd magnetic refrigeration material is 3.4 J kg. -1 K -1 .
[0069] To further demonstrate the magnetocaloric properties of Nd-Fe-Pd magnetic refrigeration materials, according to formula 2,
[0070]
[0071] Another important parameter for evaluating the magnetocaloric effect is the cooling capacity RC of the magnetocaloric material; T1 and T2 are the temperatures at the cold and hot ends corresponding to the half-width of the magnetic entropy change versus temperature curve, respectively. The maximum cooling energy RC of the Nd-Fe-Pd magnetocaloric refrigeration material under a magnetic field change of 0-5T is 220 J / kg.
[0072] The aforementioned tests have demonstrated that annealing treatment has a decisive influence on the phase composition of Nd-Fe-Pd magnetic refrigeration materials. To further demonstrate the influence of annealing conditions on Nd-Fe-Pd magnetic refrigeration materials, Comparative Examples 1, 2, and 3 are provided. Specifically, for comparison with strip spinning followed by annealing, Comparative Examples 1 and 2 used the same annealing parameters as in existing literature 4 in the background art, with annealing times of 2 hours and 4 hours respectively for the Nd-Fe-Pd magnetic refrigeration materials prepared. For comparison with direct ingot annealing, Comparative Example 3 used the same annealing parameters as in existing literature 1 and 2 in the background art, with an annealing time of 8 days for the Nd-Fe-Pd magnetic refrigeration material prepared.
[0073] Comparative Example 1
[0074] A method for preparing Nd-Fe-Pd magnetic refrigeration material with an annealing time of 2 hours is described. The steps not specifically described are the same as those in Example 1, except that in step 3, the annealing time is 2 hours, and the resulting material is referred to as Nd-Fe-Pd-2h.
[0075] To verify the crystal structure and phase composition of Nd-Fe-Pd-2h, XRD tests were performed. The XRD test results are as follows: Figure 9 As shown, in addition to the presence of the main phase Nd6Fe 13 In addition to Pd, there is also the heterogeneous phase Nd2Fe. 17 .
[0076] Comparative Example 2
[0077] A method for preparing Nd-Fe-Pd magnetic refrigeration material with an annealing time of 4h is described. The steps not specifically described are the same as those in Example 1, except that in step 3, the annealing time is 4h, and the resulting material is referred to as Nd-Fe-Pd-4h.
[0078] To verify the crystal structure and phase composition of Nd-Fe-Pd-4h, XRD tests were performed. The XRD test results are as follows: Figure 10 As shown, in addition to the presence of the main phase Nd6Fe 13 In addition to Pd, there is also the impurity phase Nd2Fe. 17 .
[0079] Comparative Examples 1 and 2 show that, according to the conditions in existing literature where annealing time is controlled in hours, impurity phase Nd2Fe will be generated. 17 Single-phase Nd-Fe-Pd magnetic refrigeration materials cannot be obtained. The reason is that Nd6Fe... 13 Pd is produced by peritectic reaction at 823K. When the annealing time is too long, a reversible peritectic reaction occurs, resulting in the formation of Nd2Fe. 17 .
[0080] Comparative Example 3
[0081] A method for preparing an Nd-Fe-Pd magnetic refrigeration material with an annealing time of 8 days is described. The steps not specifically described are the same as those in Example 1, except that in step 3, the annealing time is 8 days, and the resulting material is referred to as Nd-Fe-Pd-8D.
[0082] To verify the crystal structure and phase composition of Nd-Fe-Pd-8D, XRD tests were performed. The XRD test results are as follows: Figure 11As shown, in addition to the presence of the main phase Nd6Fe 13 In addition to Pd, there is also the impurity phase Nd2Fe. 17 and Nd5Fe 17 .
[0083] Analysis of the conclusions of Comparative Example 1 and Comparative Example 1 shows that, according to common knowledge in the art, in order to obtain a single-phase structure, even extending the annealing time to a week still cannot obtain a single-phase Nd-Fe-Pd magnetic refrigeration material with uniform composition.
[0084] Therefore, based on Comparative Examples 1, 2, and 3, it can be seen that none of the technical solutions in the existing literature can achieve the acquisition of single-phase Nd-Fe-Pd alloy magnetic refrigeration materials.
[0085] To demonstrate the effect of the spinning speed on Nd-Fe-Pd magnetic refrigeration materials, Comparative Examples 4 and 5 are provided, with Nd-Fe-Pd magnetic refrigeration materials prepared at spinning speeds of 25 m / s and 35 m / s, respectively.
[0086] Comparative Example 4
[0087] A method for preparing Nd-Fe-Pd magnetic refrigeration material with a spinning speed of 25 m / s. The steps not specifically described are the same as those in Example 1, except that in step 2, the spinning speed is 25 m / s, and the resulting material is referred to as Nd-Fe-Pd-25.
[0088] XRD analysis was performed to verify the phase composition of the obtained product. The XRD results are as follows: Figure 12 As shown, in addition to the presence of the main phase Nd6Fe 13 In addition to Pd, there is also the heterogeneous phase Nd2Fe. 17 .
[0089] Comparative Example 5
[0090] A method for preparing Nd-Fe-Pd magnetic refrigeration material with a spinning speed of 35 m / s is disclosed. Unless otherwise specified, the steps are the same as those in Example 1, except that step 2 involves the preparation of the Nd-Fe-Pd alloy thin strip. The resulting material, with a spinning speed of 35 m / s, is abbreviated as Nd-Fe-Pd-35.
[0091] XRD analysis was performed to verify the phase composition of the obtained product. The XRD results are as follows: Figure 13 As shown, in addition to the presence of the main phase Nd6Fe 13 In addition to Pd, there is also the impurity phase Nd2Fe. 17 And a small amount of amorphous material.
[0092] Analysis of the conclusions from comparing Example 1, Comparative Examples 4 and 5 shows that when the spinning speed is slow, the resulting grain size is large. Further annealing will lead to further grain enlargement, making it difficult to completely eliminate Nd₂Fe₂. 17 Impurities; when the ribbon spinning speed is too fast, the amorphous content in the ribbon increases. The increase in amorphous content directly leads to an increase in crystallization temperature, which means that complete crystallization cannot be achieved when annealing at 823K, and Nd2Fe cannot be completely eliminated. 17 The technical effect of impurities. Therefore, the belt-spinning speed has a decisive influence on achieving the technical effect.
Claims
1. A single-phase Nd-Fe-Pd alloy magnetic refrigeration material based on a rapid annealing process, characterized in that: Nd-Fe-Pd alloy thin strips are obtained by spinning Nd-Fe-Pd alloy ingots, and then Nd-Fe-Pd magnetic refrigeration materials are obtained by rapid annealing. The Nd-Fe-Pd magnetic refrigeration material is composed of single-phase Nd6Fe. 13 Pd has a tetragonal crystal structure and its space group is I4 / mcm; Its preparation method includes the following steps: Step 1, smelting of Nd-Fe-Pd alloy ingots, firstly, according to the chemical formula Nd6Fe 13 Pd, Nd, Fe, and Pd are weighed as raw materials, first cleaned with high-purity argon gas, then smelted under certain conditions by tumbling, and finally cooled to room temperature in the furnace to obtain Nd6Fe. 13 Pd alloy ingots, abbreviated as Nd-Fe-Pd alloy ingots; In step 1, the amount of Nd added needs to be increased by 2 wt.% on top of the theoretical content as compensation for loss; The cleaning conditions are as follows: a vacuum degree ≤ 2 × 10⁻⁶. -3 Under the condition of Pa, clean with high-purity argon gas 2-3 times; The conditions for the inversion melting are: the protective gas is high-purity argon, the gas pressure is 1 bar, and the number of melting times is 3. Step 2, preparation of Nd-Fe-Pd alloy thin strips: First, the Nd-Fe-Pd alloy ingot obtained in Step 1 is heated to a liquid state. Then, it is vacuum-spinned under certain conditions to obtain Nd6Fe. 13 Pd alloy thin strips are simply referred to as Nd-Fe-Pd alloy thin strips; In step 2, the vacuum belt spinning condition is that the spinning speed is 30 m / s; Step 3: Annealing of Nd-Fe-Pd alloy strips. Under certain conditions, the Nd-Fe-Pd alloy strips obtained in Step 2 are annealed to obtain Nd6Fe. 13 Pd alloy magnetic refrigeration material, abbreviated as Nd-Fe-Pd magnetic refrigeration material; In step 3, the annealing conditions are: annealing temperature of 823 K, annealing time of 5 min, and immediately after annealing, the Nd-Fe-Pd alloy strip is placed in an ice-water mixture to be rapidly cooled to room temperature.
Citation Information
Patent Citations
Nano-crystal composite NdFeB permanent magnet alloy and heating processing technology for improving magnetic performance thereof
CN101894645A
Nanoscale textured rare-earth permanent magnet material and preparation method thereof
CN111554504A