Converter continuous casting production method of high manganese austenitic steel

By optimizing key technical parameters during the converter, refining, and continuous casting processes, the problems of uneven distribution of solute elements and complex protective slag design in the casting of high-manganese austenitic steel were solved, enabling smooth continuous casting of high-manganese austenitic steel and improving the quality of the billet.

CN117587185BActive Publication Date: 2026-11-24BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311336219.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-16
Publication Date
2026-11-24
Estimated Expiration
2043-10-16

AI Technical Summary

Technical Problem

The casting process of high-manganese austenitic steel is difficult, with problems such as uneven distribution of solute elements during solidification, severe macroscopic segregation, and complex design of crystallizer taper and protective slag, which leads to decreased mechanical properties and frequent production accidents.

Method used

Optimize key technical parameters during converter, refining and continuous casting processes, including full torpedo production, enhanced tundish baking, optimized crystallizer cooling, and adjustments to alloying processes and the use of protective slag, to ensure uniform alloy composition and billet quality.

Benefits of technology

This has enabled smooth continuous casting production of high-manganese austenitic steel, improved billet quality and production efficiency, and reduced surface defects and production accidents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117587185B_ABST
    Figure CN117587185B_ABST
Patent Text Reader

Abstract

This invention discloses a converter continuous casting production method for high-manganese austenitic steel, and establishes optimized key technical parameters for the converter, refining, and continuous casting processes. The purpose of this invention is to provide a converter continuous casting production method for high-manganese austenitic steel that ensures the internal and external quality of the high-manganese steel billet while significantly improving production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metallurgical continuous casting technology, and in particular to a converter continuous casting production method for high-manganese austenitic steel. Background Technology

[0002] High-manganese steel, also known as Hadfield steel, was invented by Robert Hadfield in 1882. This steel possesses high plasticity, high toughness, and strong work hardening ability, making it an excellent wear-resistant material widely used worldwide. High-manganese steel is primarily formed by casting, although forging is also possible, but in smaller quantities. Castings using high-manganese steel generally require forging at temperatures above 1000 degrees Celsius and water quenching. While ordinary steel would typically break or melt under such water quenching, high-manganese steel undergoes rapid work hardening on its surface layer under strong impact or compression, exhibiting high wear resistance and maintaining high plasticity and toughness both internally and externally. Therefore, utilizing this characteristic, castings using high-manganese steel as the base material are particularly suitable for impact-wear conditions, such as jaw crusher jaw plates, ball mill liners, cone crusher liners, excavator buckets and teeth, and impact crusher hammers. Furthermore, railway frogs subjected to repeated impacts are also traditionally made of high-manganese steel. With increasing user demands for wear resistance and the superior performance characteristics of high-manganese steel, the demand for high-manganese steel is gradually growing. Major domestic steel mills have begun to focus on its research and development, but production is severely limited by the fact that high-manganese steel can only be die-cast. However, the high Mn and Al content of high-manganese austenitic steel makes its casting process exceptionally difficult. Both primary and secondary cooling in continuous casting require special designs to ensure the caster shell reaches a safe thickness and that the temperature drop during casting is controlled, preventing defects such as bulging and cracking during solidification. Due to its high Mn and Al content and wide solid-liquid two-phase region, selective crystallization occurs during solidification, resulting in uneven distribution of solute elements in the solidified structure. This leads to severe macroscopic segregation, reducing mechanical properties, particularly toughness, plasticity, and corrosion resistance. Furthermore, the transformation from δ-ferrite to γ-austenite during continuous casting solidification causes significant volume shrinkage, necessitating special design for the crystallizer taper and the performance of the protective slag to avoid surface defects such as dents and cracks, and even leaks. Meanwhile, due to the high Al content, Al will react with functional refractory materials such as stoppers, submerged nozzles, covering agents, and protective slags during the casting process, which will cause the original functional refractory materials to degenerate and lose their original functionality, leading to production and quality accidents. Summary of the Invention

[0003] The purpose of this invention is to provide a converter continuous casting production method for high-manganese austenitic steel, which ensures the internal and external quality of the high-manganese steel billet and greatly improves production efficiency.

[0004] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0005] This invention discloses a converter continuous casting production method for high-manganese austenitic steel. Optimized key technical parameters have been established for the converter, refining, and continuous casting processes. The method specifically includes the following steps:

[0006] 1) Converter process

[0007] To ensure the molten iron is produced using a full torpedo production process, avoiding waiting for iron to be added, the molten iron undergoes desulfurization pretreatment, and the [S] content of the molten iron entering the furnace is ≤0.015%. Slag is removed before and after treatment, and removed until a mirror finish is achieved. High-speed pulling and supplementary blowing operations are employed, and the phosphorus content at tapped steel is less than 0.020%. The tapping temperature of the converter is required to be ≥1680℃. Oxygen is determined before tapping, and the ladle argon blowing device is checked before tapping to ensure good double-line argon blowing in the ladle. The converter process uses metallic manganese deoxidation and alloying, and the steel is added to the hopper before tapping. Add metallic manganese as needed, and add coke according to the final carbon content. Starting from 1 / 4 of the steel is tapped, silicon, calcium, and barium are added from the back of the furnace for deoxidation and alloying. For argon blowing during tapping, the converter and ladle repair department confirm that argon blowing in the ladle is on before tapping. Use double-line argon blowing during tapping. When the steel volume is greater than 2 / 3, the argon volume is halved. If the argon blowing is weak during tapping, contact the ladle repair department immediately. After tapping, the ladle car is placed back in the furnace and double-line argon blowing continues for 2-4 minutes. Use the converter sliding plate to block slag during tapping, adopting a double-sliding mode, and slag is not allowed to fall.

[0008] 2) Refining process

[0009] The converter ensures a sufficient steel output to allow for both refining heating and subsequent alloy addition. The ladle maintains a slight positive pressure throughout the process. Heating begins based on the top slag condition upon entry, with argon gas ensuring a 300mm blowing area. 300kg of refining quicklime is added, along with metallic manganese. When Mn and Al content is high, a portion of the alloy is first melted in a smelting furnace and then poured into the refining LF furnace to shorten smelting time. Calcium carbide is added during refining heating, and after heating, the slag is dipped in slag, with the slag material adjusted according to viscosity. If the composition is insufficient, more quicklime is added. After heating stops, the slag layer is observed; if insufficient, more quicklime is added. Vacuum degassing (VD) is performed, with deep vacuum pressure held for at least 20 minutes, before being hoisted back to the refining furnace for continued Al addition. Refining is adjusted based on Al content; no calcium treatment is performed.

[0010] 3) Continuous casting process

[0011] Use a crystallizer with a suitable taper, employ weak primary cooling, and a secondary cooling water flow rate of 3100 L / min to ensure a 4-6℃ temperature difference between the inlet and outlet water. Strengthen the baking process of the tundish to increase the temperature of the functional refractory material in the tundish before casting, preventing Al2O3 inclusions in the molten steel from adsorbing and accumulating on the submerged entry nozzle and stopper rod, which could lead to molten steel flow interruption. Maintain an ambient temperature of 1250℃-1300℃ inside the tundish before casting. Replace the gas inside the tundish with argon gas before casting to prevent Al oxidation in the molten steel during the casting process. After casting begins, protect the top of the tundish with argon gas throughout the process, and simultaneously seal the long nozzle of the ladle with argon gas. The superheat is 50-70℃ to ensure good melting of the protective slag during the initial casting process, prevent the formation of cold steel on the surface of the molten steel in the crystallizer, and avoid excessive superheat that could lead to insufficient thickness of the billet shell after initial casting, resulting in steel leakage. A longer initial casting start time is adopted to ensure that the billet shell reaches a safe thickness. The preferred process parameters are: start time 130s to 150s. A lower casting speed than that for ordinary steel grades is used during the casting process to reduce the deformation rate of the billet shell during solidification, avoid bulging deformation and surface cracks. The casting speed is adjusted according to the superheat, with a control range of 0.40-0.50m / min.

[0012] Furthermore, the chemical composition of high manganese steel is as follows: C 0.40%-1.00%, Mn 18.0%-25.0%, Al 1.50%-2.50%, Si≤0.50%, Ti 0.09-0.15%, S≤0.03%, P≤0.03%, and rare earth RE 30-100ppm.

[0013] Furthermore, in step 1), the target phosphorus content in the steel is 0.010%.

[0014] Furthermore, in step 1), the final deoxidizer used is barium silicate.

[0015] Furthermore, in step 3), the superheat is 55-65℃.

[0016] Furthermore, in step 3), a high-alkalinity protective slag with an alkalinity R = 1.4 is used.

[0017] Furthermore, in step 3), the intermediate package covering agent uses carbon-free rice husk.

[0018] Furthermore, in step 3), the dry material in the intermediate package uses a low-hydrogen, high-magnesium material.

[0019] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0020] A converter continuous casting method for high-manganese austenitic steel is provided. Through targeted improvements to converter alloying, refining, and continuous casting processes, the production of high-manganese austenitic steel in continuous casting is made smooth. Attached Figure Description

[0021] The present invention will be further described below with reference to the accompanying drawings.

[0022] Figure 1 To improve the previous billet photo;

[0023] Figure 2 Photo of the improved casting billet. Detailed Implementation

[0024] This invention patent is applied in the continuous casting production of high-manganese austenitic steel in a converter. The specific process route is: KR hot metal pretreatment—converter—LF refining—VD vacuum treatment—280×380mm large billet casting machine. The steel composition is shown in Table 1.

[0025] Table 1 Chemical composition (%) of high-manganese austenitic steel

[0026]

[0027] Desulfurization must be performed before the converter process to ensure that the sulfur content entering the furnace is within the control target. The converter charge and scrap steel addition must be strictly controlled, with a deviation within ±2 tons. High-tension blowing operation is adopted to ensure the phosphorus content of the tapped steel. The tapping temperature is controlled to create favorable conditions for refining. Alloying is performed during tapping, controlling the amount of metallic manganese added, and coke is added to increase carbon content. Specific process parameters are shown in Table 2.

[0028] Table 2 Converter parameter control status

[0029]

[0030] The refining process strictly follows the above operating procedures. After VD vacuum degassing, the ladle returns to the refining station, where Al ingots or Al granules are added; calcium treatment is not required. The continuous casting ladle baking time must be at least 300 minutes to ensure the tundish ambient temperature exceeds 1250℃. Argon gas is used to purge the gas inside the tundish during the tundish car's movement to the casting position. After casting begins, the argon purge flow in the tundish is adjusted to a minimum, with argon protection maintained throughout the process. Simultaneously, the long nozzle of the ladle is sealed with argon gas for protection. After production, the functional refractory materials in the tundish are inspected, and all meet the usage requirements.

[0031] The main production parameters for continuous casting are shown in Table 3.

[0032] Table 3 Process parameters for continuous casting

[0033]

[0034]

[0035] The production process proceeded smoothly and stably, with stable liquid level control in the tundish. After process improvements, the corner cracks of the cast billet were significantly reduced. See attached photos for details. Figure 1 and Figure 2 .

[0036] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A method for the production of high manganese austenitic steel by converter and continuous casting, in which the optimal key technological parameters are defined during the converter, refining and continuous casting production process, characterised in that, Specifically, the following steps are included: 1) Converter process To ensure the molten iron is produced using a full torpedo production process, avoiding waiting for iron to be produced, the molten iron undergoes desulfurization pretreatment, and the [S] content of the molten iron entering the furnace is ≤0.015%; slag is removed before and after treatment, and the slag is removed until the surface is mirror-like; high-pulling and supplementary blowing operations are adopted, and the phosphorus content of the tapped steel is less than 0.020%; the tapping temperature of the converter is required to be ≥1680℃; oxygen is determined before tapping, and the ladle argon blowing device is checked before tapping to ensure good double-line argon blowing in the ladle; the converter process uses metallic manganese deoxidation and alloying, and the molten iron is added from the hopper during tapping. Add metallic manganese and coke according to the final carbon content. Starting from 1 / 4 of the steel is tapped, silicon, calcium, and barium are added from the back of the furnace for deoxidation and alloying. For argon blowing during tapping, the converter and ladle repair department confirm that argon blowing in the ladle is on before tapping. Use double-line argon blowing during tapping. When the steel volume is greater than 2 / 3, the argon volume is halved. If the argon blowing is weak during tapping, contact the ladle repair department immediately. After tapping, the ladle car is moved to the back of the furnace and double-line argon blowing continues for 2-4 minutes. Use the converter sliding plate to block slag during tapping, adopting a double-sliding mode, and slag is not allowed to fall. 2) Refining process The converter ensures a sufficient steel output to allow for both refining heating and subsequent alloy addition. The ladle maintains a slight positive pressure throughout the process. Heating begins based on the top slag condition upon entry, with argon gas ensuring a 300mm blowing area. 300kg of refining quicklime is added, along with metallic manganese. When Mn and Al content is high, a portion of the alloy is first melted in a smelting furnace and then poured into the refining LF furnace to shorten smelting time. Calcium carbide is added during refining heating, and after heating, the slag is dipped in slag, with the slag material adjusted according to viscosity. If the composition is insufficient, more quicklime is added. After heating stops, the slag layer is observed; if insufficient, more quicklime is added. Vacuum degassing (VD) is performed, with deep vacuum pressure held for at least 20 minutes, before being hoisted back to the refining furnace for continued Al addition. Refining is adjusted based on Al content; no calcium treatment is performed. 3) Continuous casting process A crystallizer with a suitable taper is used, with weak primary cooling and a secondary cooling water flow rate of 3100 L / min, ensuring a 4-6℃ temperature difference between the inlet and outlet water. The tundish baking is intensified to increase the temperature of the functional refractory material in the tundish before casting, preventing Al2O3 inclusions in the molten steel from adsorbing and accumulating on the submerged entry nozzle and stopper rod, thus avoiding steel flow interruption. The ambient temperature inside the tundish before casting is 1250℃-1300℃. Argon gas is used to replace the gas inside the tundish before casting to prevent Al oxidation in the molten steel during casting. After casting begins, the top of the tundish is protected with argon gas throughout the process, while the long nozzle of the ladle is also used. Argon gas is used for sealing and protection; the superheat is 50-70℃ to ensure good melting of the protective slag during the initial casting process, to prevent cold steel from forming on the surface of the molten steel in the crystallizer, and to avoid excessive superheat causing the billet shell to not reach a safe thickness after initial casting, resulting in steel leakage; the initial casting start time is 130s to 150s to ensure that the billet shell reaches a safe thickness during initial casting; a lower casting speed than ordinary steel grades is used during the casting process to reduce the deformation rate of the billet shell during solidification, to avoid bulging deformation and surface cracks, and the casting speed is adjusted according to the superheat, with a control range of 0.40-0.50m / min.

2. The production method of high manganese austenite steel by converter continuous casting according to claim 1, characterized in that, Chemical composition of high manganese steel: C 0.40%-1.00%, Mn 18.0%-25.0%, Al 1.50%-2.50%, Si ≤0.50%, Ti 0.09-0.15%, S≤0.03%, P ≤0.03%, rare earth RE 30-100ppm.

3. The production method of high manganese austenite steel by converter continuous casting according to claim 1, characterized in that, In step 1), the target phosphorus content in the steel output is 0.010%.

4. The production method of high manganese austenite steel by converter continuous casting according to claim 1, characterized in that, In step 1), the final deoxidizer used is barium silicate.

5. The production method of high manganese austenite steel by converter continuous casting according to claim 1, characterized in that, In step 3), the superheat is 55-65℃.

6. The converter continuous casting production method for high-manganese austenitic steel according to claim 1, characterized in that, In step 3), a high-alkalinity protective slag with an alkalinity R=1.4 is used.

7. The converter continuous casting production method for high-manganese austenitic steel according to claim 1, characterized in that, In step 3), carbon-free rice husks are used as the intermediate packing covering agent.

8. The converter continuous casting production method for high-manganese austenitic steel according to claim 1, characterized in that, In step 3), the intermediate dry material uses a low-hydrogen, high-magnesium material.

Citation Information

Patent Citations

  • Smelting method of high-manganese wear-resistant steel

    CN103484599A

  • Preparation method for high-manganese steel for ocean platform and continuous casting slab of high-manganese steel

    CN105908080A