Zinc alloy negative electrode and preparation method and application thereof
By preparing zinc-tin binary alloy anodes through electrodeposition, the problems of dendrite growth and structural instability of zinc anodes were solved, enabling the application of high-efficiency zinc-tin alloy anodes in aqueous zinc-ion batteries. This improved the cycle stability and depth of discharge of the batteries, making them suitable for industrial production.
Patent Information
- Application Number
- CN202311559787.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-22
AI Technical Summary
Zinc anodes suffer from uncontrolled dendrite growth, structural instability, and poor cycle stability during charge and discharge, leading to battery short circuits and loss of active zinc, making it difficult to maintain efficient and reversible zinc deposition behavior during long-term cycling.
A zinc-tin binary alloy anode was prepared by electrodeposition. By controlling the molar ratio of zinc and tin in the electrolyte and the current density during the electrodeposition process, a zinc-tin alloy coating with a highly oriented (002) crystal plane was formed, thereby improving the structural stability and ionic conductivity of the zinc-tin alloy anode.
This study achieves excellent cycle stability and depth of discharge for zinc-tin alloy anodes at high current densities, simplifies the preparation process, and makes them suitable for the industrial production of aqueous zinc-ion batteries.
Smart Images

Figure CN117587474B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of aqueous zinc metal battery technology, specifically relating to a zinc alloy negative electrode, its preparation method, and its application. Background Technology
[0002] Rechargeable aqueous zinc-ion batteries (AZIBs) have emerged as candidates for emerging energy storage devices due to their advantages such as high safety, environmental friendliness, low cost, and high capacity. Zinc, as the negative electrode, possesses inherent advantages: compared to other active metal negative electrodes, metallic zinc exhibits higher stability in aqueous media and humid atmospheres, allowing for direct assembly of zinc batteries under unprotected atmospheres; a moderate standard electrode potential (-0.762V vs. SHE) and a high hydrogen evolution overpotential ensure efficient and reversible zinc deposition / stripping behavior; and the two-electron transfer redox reaction endows metallic zinc with higher volumetric and gravimetric specific capacities, at 5855 mAh cm⁻¹. -3 and 820mAh g -1 .
[0003] However, zinc anodes still face many key challenges: uncontrolled zinc dendrites can puncture the glass fiber separator, ultimately leading to a short circuit; preferential dissolution at the dendrite roots can cause the dendrites to separate from the host, resulting in "dead zinc" that loses its activity and accelerates zinc consumption. Furthermore, due to the inherent hostless nature of zinc anodes, they easily become unstable after repeated cycling. These structural defects are irreparable, significantly increasing the risk of battery failure. Therefore, developing anode materials with uniform zinc deposition behavior is of great significance for improving the overall performance of AZIBs.
[0004] In recent years, numerous researchers have proposed various solutions from the anode side, including constructing interfacial protective layers and designing three-dimensional structures. While these strategies can improve the performance of zinc metal anodes to some extent, they are difficult to sustain during long-term cycling. Specifically, in-situ and ex-situ coatings are only effective on the surface and struggle to maintain interfacial integrity during cycling; three-dimensional structures require complex fabrication processes, and the structural network is prone to deformation and even collapse. Currently, there is an urgent need to explore substantial modification measures to fundamentally address the thermodynamic and kinetic challenges faced by zinc anodes.
[0005] Zinc has a hexagonal close-packed (hcp) structure, and the atomic structure of different crystal planes varies greatly. Among them, the (002) crystal plane has the lowest surface energy, which induces the deposition of the (002) crystal plane, which is conducive to the formation of a flat morphology and inhibits dendrite growth. At present, most researchers use electrolyte additives to control the preferred orientation of zinc (002) crystal planes, but the improvement of (002) crystal plane strength is small and too one-sided, without considering the impact of additives on cathode materials and the battery as a whole. The corrosion reaction of zinc anode under weakly acidic conditions is mainly controlled by hydrogen evolution. When two metals bond to each other, the dissolution potential of non-noble metals will shift positively. Therefore, alloying with high hydrogen overpotential metals (such as tin, indium, etc.) can effectively improve the corrosion resistance of zinc alloys. Liu Hong's team used a simple displacement reaction to immerse zinc sheets in tin salt solution to obtain anodes with zinc-tin alloy interfaces, but the tin content is uncontrollable and the surface is not uniform under this method. Summary of the Invention
[0006] To address the serious side reactions that occur in existing zinc anodes during charging and discharging, resulting in low coulombic efficiency and poor cycle stability, this invention provides a zinc alloy anode, its preparation method, and its application. By combining preferred orientation with alloying, and by simply controlling the electroplating solution and electrodeposition process, a zinc-tin binary alloy coating with certain characteristics and areal capacity can be unexpectedly obtained. A zinc-tin alloy anode with a highly oriented (002) crystal plane is prepared in one step and used as the reaction surface of an aqueous zinc metal battery, exhibiting excellent electrochemical performance.
[0007] To achieve the above-mentioned technical objectives, the present invention adopts the following technical solution:
[0008] A method for preparing a zinc alloy negative electrode involves mixing zinc salt, tin salt, a complexing agent, and water to obtain an electroplating solution; under constant current mode, the electroplating solution is electrodeposited on the surface of a substrate to obtain a zinc-tin binary alloy coating, wherein the molar ratio of the zinc salt to the tin salt is 40 to 20:1.
[0009] Preferably, the zinc salt is ZnSO4·7H2O, ZnCl2 or Zn(CF3SO3)2, and the tin salt is SnSO4 or SnCl2; the concentration of the zinc salt in the electroplating solution is 0.1 to 1 mol / L.
[0010] Preferably, the complexing agent is EDTA-2Na, and its concentration in the electroplating solution is 0.01 to 0.1 mol / L.
[0011] Preferably, the substrate is copper foil, zinc foil, titanium foil, or carbon-based material.
[0012] Preferably, the current density of the electrodeposition is 5–30 mA / cm². 2 Further preferred is 10–20 mA / cm 2 .
[0013] Preferably, the electrodeposition process is as follows: using a zinc sheet as the negative electrode and a copper sheet as the positive electrode, constant current electrodeposition is performed in an electrolytic cell to deposit a zinc-tin binary alloy plating layer on the copper sheet.
[0014] The present invention also provides a zinc alloy negative electrode prepared by the above preparation method, wherein the (002) crystal plane of the Zn phase is the main orientation, and the weight percentage content of Zn and Sn is 85-95:5-15.
[0015] This invention also provides an application of the above-mentioned zinc alloy negative electrode, which is used to prepare aqueous zinc metal batteries.
[0016] The advantages of this invention are:
[0017] (1) This invention innovatively proposes a method for preparing zinc-tin alloy composite anode material with strong (002) orientation in one step based on electrodeposition. By means of the synergistic control of the zinc-tin molar ratio in the electrolyte and the current density in the electrodeposition process, a zinc-tin binary alloy coating with high structural stability, ionic conductivity and good substrate bonding can be formed on the substrate surface. Based on this simple preparation method, the preferred orientation of the (002) crystal plane can be obtained, which helps to further improve the discharge depth and cycle stability under high current density of the composite anode.
[0018] (2) Compared with many high-energy-consuming synthesis routes, the preparation method of zinc alloy-induced coating modified zinc anode provided by the present invention is simple, efficient and time-saving, which is conducive to the large-scale industrial production of aqueous zinc-ion batteries. Attached Figure Description
[0019] Figure 1 The XRD patterns are those of Zn|Sn-1 in Example 1, Zn-1 in Comparative Example 1, and Bare Zn in Comparative Example 3.
[0020] Figure 2 The XRD patterns are of Zn|Sn-2 in Example 2, Zn-2 in Comparative Example 2, and Bare Zn in Comparative Example 3.
[0021] Figure 3 The XRD patterns are of Zn|Sn-1 in Example 1, Zn|Sn-3 in Example 3, and Zn|Sn-4 in Example 4.
[0022] Figure 4 XRD patterns of Zn|Sn-1 in Example 1, Zn|Sn-5 in Comparative Example 4, and Zn|Sn-6 in Comparative Example 5 (a); and a photograph of the deposited coating of Zn|Sn-5 in Comparative Example 4 (b).
[0023] Figure 5 The image shows the electroplating solution and the deposited coating used for Zn|Sn-6 in Comparative Example 6.
[0024] Figure 6 The chemical composition of Zn|Sn-1 in Example 1 and Zn|Sn-2 in Example 2, as determined by inductively coupled plasma atomic emission spectrometry (ICP).
[0025] Figure 7 The scan images are of the deposited negative electrodes obtained in Examples 1(a), 2(b), 1(c), and 2(d).
[0026] Figure 8 Comparison of the zinc / zinc symmetric battery cycle performance of Zn|Sn-1 in Example 1, Zn-1 in Comparative Example 1, and Bare Zn in Comparative Example 3 (a); Comparison of the zinc / zinc symmetric battery cycle performance of Zn|Sn-2 in Example 2, Zn-2 in Comparative Example 2, and Bare Zn in Comparative Example 3 (b).
[0027] Figure 9 XRD patterns of the Zn|Sn-1 symmetrical battery of Example 1 after cycling for the corresponding number of cycles (a); SEM image of the negative electrode side after 50 cycles (b); SEM image of the negative electrode side after 80 cycles (c).
[0028] Figure 10 The graph shows a comparison of the electrochemical performance of Zn|Sn-1 from Example 1, Zn|Sn-2 from Example 2, and Bare Zn from Comparative Example 3 using ammonium vanadate cathode. Detailed Implementation
[0029] The present invention will be further described below with reference to the accompanying drawings and embodiments. The raw materials described in the present invention are all obtained through commercial means. Unless otherwise specified, the preparation methods described in the present invention are conventional preparation methods in the art. The following embodiments are intended to illustrate the present invention and not to further limit the present invention.
[0030] Example 1
[0031] A method for preparing a zinc-tin binary alloy anode with (002) orientation electrodeposited on a copper substrate includes the following steps:
[0032] Step 1: Weigh 11.55024g of zinc sulfate heptahydrate ZnSO4·7H2O, 0.42954g of stannous sulfate SnSO4, and 1.8612g of disodium ethylenediaminetetraacetate EDTA-2Na, add them to 100ml of deionized water, stir and dissolve at room temperature to obtain the electroplating solution.
[0033] Step 2: Cut the initial copper foil and zinc foil to obtain copper sheets (8cm*8cm) and zinc sheets (8cm*8cm) of fixed size that can be put into the electrolytic tank. Then, perform surface treatment on the copper sheets and zinc sheets, remove any dust, oil, oxides, etc. that may be present with alcohol, and place them in the plating tank after rinsing with deionized water.
[0034] Step 3: Select a constant current of 20mA / cm -2 The electroplating time is 15 minutes for the electrodeposition process.
[0035] Step 4: After electrodeposition, remove the positive electrode deposition side, rinse with deionized water, dry in a drying oven, and then remove to obtain Zn|Sn-1 with a deposition surface capacity of 5 mAh cm⁻¹. -2 ;
[0036] Step 5: Using a tablet press, the electroplated layer, along with the copper substrate, is punched into a 15mm diameter disc for use as the negative electrode of the zinc-ion battery, where the deposited layer serves as the reaction surface of the battery.
[0037] Example 2
[0038] A method for preparing a zinc-tin binary alloy anode with (002) orientation electrodeposited on a copper substrate includes the following steps:
[0039] Step 1: Weigh 11.5504g of zinc sulfate heptahydrate ZnSO4·7H2O, 0.21477g of stannous sulfate SnSO4, and 1.8612g of disodium ethylenediaminetetraacetate EDTA-2Na, add them to 100ml of deionized water, stir and dissolve at room temperature to obtain the electroplating solution.
[0040] Step 2: Cut the initial copper foil and zinc foil to obtain copper sheets (8cm*8cm) and zinc sheets (8cm*8cm) of fixed size that can be put into the electrolytic tank. Then, perform surface treatment on the copper sheets and zinc sheets, remove any dust, oil, oxides, etc. that may be present with alcohol, and place them in the plating tank after rinsing with deionized water.
[0041] Step 3: Select a constant current of 10mA / cm -2 The electroplating time is 30 minutes for the electrodeposition process.
[0042] Step 4: After electrodeposition, remove the positive electrode deposition side, rinse with deionized water, dry in a drying oven, and then remove to obtain Zn|Sn-2 with a deposition surface capacity of 5 mAh cm⁻². -2 ;
[0043] Step 5: Using a tablet press, the electroplated layer, along with the copper substrate, is punched into a 15mm diameter disc for use as the negative electrode of the zinc-ion battery, with the deposited layer serving as the reaction surface of the battery.
[0044] Example 3
[0045] A method for preparing a zinc-tin binary alloy negative electrode by electrodeposition on a copper substrate includes the following steps:
[0046] Step 1: Weigh 11.55024g of zinc sulfate heptahydrate ZnSO4·7H2O, 0.42954g of stannous sulfate SnSO4, and 1.8612g of disodium ethylenediaminetetraacetate EDTA-2Na, add them to 100ml of deionized water, stir and dissolve at room temperature to obtain the electroplating solution.
[0047] Step 2: Cut the initial copper foil and zinc foil to obtain copper sheets (8cm*8cm) and zinc sheets (8cm*8cm) of fixed size that can be put into the electrolytic tank. Then, perform surface treatment on the copper sheets and zinc sheets, remove any dust, oil, oxides, etc. that may be present with alcohol, and place them in the plating tank after rinsing with deionized water.
[0048] Step 3: Select a constant current of 5mA / cm -2 The electroplating time is 60 minutes for the electrodeposition process.
[0049] Step 4: After electrodeposition, remove the positive electrode deposition side, rinse with deionized water, dry in a drying oven, and then remove to obtain Zn|Sn-3 with a deposition surface capacity of 5 mAh cm⁻¹. -2 ;
[0050] Step 5: Using a tablet press, the electroplated layer, along with the copper substrate, is punched into a 15mm diameter disc for use as the negative electrode of the zinc-ion battery, with the deposited layer serving as the reaction surface of the battery.
[0051] Example 4
[0052] A method for preparing a zinc-tin binary alloy negative electrode by electrodeposition on a copper substrate includes the following steps:
[0053] Step 1: Weigh 11.55024g of zinc sulfate heptahydrate ZnSO4·7H2O, 0.42954g of stannous sulfate SnSO4, and 1.8612g of disodium ethylenediaminetetraacetate EDTA-2Na, add them to 100ml of deionized water, stir and dissolve at room temperature to obtain the electroplating solution.
[0054] Step 2: Cut the initial copper foil and zinc foil to obtain copper sheets (8cm*8cm) and zinc sheets (8cm*8cm) of fixed size that can be put into the electrolytic tank. Then, perform surface treatment on the copper sheets and zinc sheets, remove any dust, oil, oxides, etc. that may be present with alcohol, and place them in the plating tank after rinsing with deionized water.
[0055] Step 3: Select a constant current of 30mA / cm -2The electroplating time is 10 minutes, and the electrodeposition process is carried out.
[0056] Step 4: After electrodeposition, remove the positive electrode deposition side, rinse with deionized water, dry in a drying oven, and then remove to obtain Zn|Sn-4 with a deposition surface capacity of 5 mAh cm⁻¹. -2 ;
[0057] Step 5: Using a tablet press, the electroplated layer, along with the copper substrate, is punched into a 15mm diameter disc for use as the negative electrode of the zinc-ion battery, with the deposited layer serving as the reaction surface of the battery.
[0058] Comparative Example 1
[0059] A method for preparing a zinc metal anode by electrodeposition on a copper substrate includes the following steps:
[0060] Step 1: Weigh 11.5504g of zinc sulfate heptahydrate ZnSO4·7H2O and 1.8612g of disodium ethylenediaminetetraacetate EDTA-2Na, add them to 100ml of deionized water, stir and dissolve at room temperature to obtain the electroplating solution.
[0061] Step 2: Cut the initial copper foil and zinc foil to obtain copper and zinc sheets of fixed size that can be put into the electrolytic cell. Then, perform surface treatment on the copper and zinc sheets, remove any dust, oil, oxides, etc. that may be present with alcohol, and place them in the plating tank after rinsing with deionized water.
[0062] Step 3: Select a constant current of 20mA / cm -2 The electroplating time is 15 minutes for the electrodeposition process.
[0063] Step 4: After electrodeposition, remove the positive electrode deposition side, rinse with deionized water, dry in a drying oven, and then remove to obtain Zn-1 with a deposition areal capacity of 5 mAh cm⁻¹. -2 ;
[0064] Step 5: Using a tablet press, the electroplated layer, along with the copper substrate, is punched into a 15mm diameter disc for use as the negative electrode of the zinc-ion battery, with the deposited layer serving as the reaction surface of the battery.
[0065] Comparative Example 2
[0066] A method for preparing a zinc metal anode by electrodeposition on a copper substrate includes the following steps:
[0067] Step 1: Weigh 11.5504g of zinc sulfate heptahydrate ZnSO4·7H2O and 1.8612g of disodium ethylenediaminetetraacetate (EDTA-2Na), add them to 100ml of deionized water, stir and dissolve at room temperature to obtain the electroplating solution.
[0068] Step 2: Cut the initial copper foil and zinc foil to obtain copper and zinc sheets of fixed size that can be put into the electrolytic cell. Then, perform surface treatment on the copper and zinc sheets, remove any dust, oil, oxides, etc. that may be present with alcohol, and place them in the plating tank after rinsing with deionized water.
[0069] Step 3: Select a constant current of 10mA / cm -2 The electroplating time is 30 minutes for the electrodeposition process.
[0070] Step 4: After electrodeposition, remove the positive electrode deposition side, rinse with deionized water, dry in a drying oven, and then remove to obtain Zn⁻⁂ with a deposition areal capacity of 5 mAh cm⁻¹. -2 ;
[0071] Step 5: Using a tablet press, the electroplated layer, along with the copper substrate, is punched into a 15mm diameter disc for use as the negative electrode of the zinc-ion battery, with the deposited layer serving as the reaction surface of the battery.
[0072] Comparative Example 3
[0073] Ordinary zinc sheets (Bare Zn) with a thickness of 10 micrometers were used. The zinc sheets were purchased from Weifang Purun Co., Ltd., and have a zinc content of over 99.9%. The sheet surface capacity is approximately 5 mAh cm³. -2 A tablet press is used to punch out 15mm diameter discs for use as the negative electrode in zinc-ion batteries.
[0074] Comparative Example 4
[0075] A method for preparing a zinc-tin binary alloy negative electrode by electrodeposition on a copper substrate includes the following steps:
[0076] Step 1: Weigh 11.55024g of zinc sulfate heptahydrate ZnSO4·7H2O, 0.64431g of stannous sulfate SnSO4, and 1.8612g of disodium ethylenediaminetetraacetate EDTA-2Na, add them to 100ml of deionized water, stir and dissolve at room temperature to obtain the electroplating solution.
[0077] Step 2: Cut the initial copper foil and zinc foil to obtain copper sheets (8cm*8cm) and zinc sheets (8cm*8cm) of fixed size that can be put into the electrolytic tank. Then, perform surface treatment on the copper sheets and zinc sheets, remove any dust, oil, oxides, etc. that may be present with alcohol, and place them in the plating tank after rinsing with deionized water.
[0078] Step 3: Select a constant current of 20mA / cm -2 The electroplating time is 15 minutes for the electrodeposition process.
[0079] Step 4: After electrodeposition, remove the positive electrode deposition side, rinse with deionized water, dry in a drying oven, and then remove to obtain Zn|Sn-5 with a deposition surface capacity of 5 mAh cm⁻¹. -2 ;
[0080] Step 5: Using a tablet press, the electroplated layer, along with the copper substrate, is punched into a 15mm diameter disc for use as the negative electrode of the zinc-ion battery, with the deposited layer serving as the reaction surface of the battery.
[0081] Comparative Example 5
[0082] A method for preparing a zinc-tin binary alloy negative electrode by electrodeposition on a copper substrate includes the following steps:
[0083] Step 1: Weigh 11.55024g of zinc sulfate heptahydrate ZnSO4·7H2O, 0.10739g of stannous sulfate SnSO4, and 1.8612g of disodium ethylenediaminetetraacetate EDTA-2Na, add them to 100ml of deionized water, stir and dissolve at room temperature to obtain the electroplating solution.
[0084] Step 2: Cut the initial copper foil and zinc foil to obtain copper sheets (8cm*8cm) and zinc sheets (8cm*8cm) of fixed size that can be put into the electrolytic tank. Then, perform surface treatment on the copper sheets and zinc sheets, remove any dust, oil, oxides, etc. that may be present with alcohol, and place them in the plating tank after rinsing with deionized water.
[0085] Step 3: Select a constant current of 20mA / cm -2 The electroplating time is 15 minutes for the electrodeposition process.
[0086] Step 4: After electrodeposition, remove the positive electrode deposition side, rinse with deionized water, dry in a drying oven, and then remove to obtain Zn|Sn-6 with a deposition surface capacity of 5 mAh cm⁻¹. -2 ;
[0087] Step 5: Using a tablet press, the electroplated layer, along with the copper substrate, is punched into a 15mm diameter disc for use as the negative electrode of the zinc-ion battery, with the deposited layer serving as the reaction surface of the battery.
[0088] Comparative Example 6
[0089] A method for preparing a zinc-tin binary alloy negative electrode by electrodeposition on a copper substrate includes the following steps:
[0090] Step 1: Weigh 11.55024g of zinc sulfate heptahydrate ZnSO4·7H2O and 0.10739g of stannous sulfate SnSO4, add them to 100ml of deionized water, stir and dissolve at room temperature to obtain the electroplating solution;
[0091] Step 2: Cut the initial copper foil and zinc foil to obtain copper sheets (8cm*8cm) and zinc sheets (8cm*8cm) of fixed size that can be put into the electrolytic tank. Then, perform surface treatment on the copper sheets and zinc sheets, remove any dust, oil, oxides, etc. that may be present with alcohol, and place them in the plating tank after rinsing with deionized water.
[0092] Step 3: Select a constant current of 20mA / cm -2 The electroplating time is 15 minutes for the electrodeposition process.
[0093] Step 4: After electrodeposition, remove the positive electrode deposition side, rinse with deionized water, dry in a drying oven, and then remove to obtain Zn|Sn-7 with a deposition surface capacity of 5 mAh cm⁻¹. -2 ;
[0094] Step 5: Using a tablet press, the electroplated layer, along with the copper substrate, is punched into a 15mm diameter disc for use as the negative electrode of the zinc-ion battery, with the deposited layer serving as the reaction surface of the battery.
[0095] like Figure 1 The figures show the XRD patterns of Example 1 (Zn|Sn-1), Comparative Example 1 (Zn-1), and Comparative Example 3 (Bare Zn). Comparative Example 1 (Zn-1) deposited zinc metal, and the (002) orientation of the deposited zinc metal was significantly improved compared to ordinary commercially available zinc sheets (Bare Zn). In Example 1 (Zn|Sn-1), four lower peaks appeared corresponding to the Sn phase (PDF#04-0673), and the peak value of the (002) crystal plane of the Zn phase was significantly enhanced.
[0096] like Figure 2 The figures show the XRD patterns of Example 2 (Zn|Sn-2), Comparative Example 2 (Zn-2), and Comparative Example 3 (Bare Zn). Comparative Example 1 (Zn-2) deposited zinc metal, and the (002) orientation of the deposited zinc metal was significantly improved compared to ordinary commercially available zinc sheets (Bare Zn). In Example 2 (Zn|Sn-2), four lower peaks appeared corresponding to the Sn phase (PDF#04-0673), and the peak value of the (002) crystal plane of the Zn phase was significantly enhanced.
[0097] like Figure 3 The image shows the XRD patterns of Examples 1 (Zn|Sn-1), 3 (Zn|Sn-3), and 4 (Zn|Sn-4) at 5-30 mA / cm². -2 (002) oriented zinc-tin binary alloys can be obtained at current densities of 10-20 mA / cm², while at current densities of 10-20 mA / cm², the desired results are achieved. -2 At that time, the peak intensity of the (002) crystal plane is better.
[0098] like Figure 4 As shown, (a) are the XRD patterns of Example 1 (Zn|Sn-1), Comparative Example 4 (Zn|Sn-5) and Comparative Example 5 (Zn|Sn-6), and (b) are the actual images of the deposited coating of Comparative Example 4 (Zn|Sn-5). When the molar ratio of zinc salt to tin salt is relatively low, although a (002) oriented zinc-tin binary alloy can be obtained, the surface of the deposited coating is covered by a loosely structured substance, resulting in low adhesion to the substrate. Such coatings are of low quality and cannot be used as anode materials for aqueous zinc-ion batteries. When the molar ratio of zinc salt to tin salt is relatively high, a (002) oriented zinc-tin alloy cannot be obtained, and the expected effect is not achieved.
[0099] like Figure 5 The image shown is a photograph of the electroplating solution and the deposited coating of Comparative Example 6 (Zn|Sn-7). Without the addition of a complex, Sn... 2+ It is extremely prone to hydrolysis in aqueous solution, which makes the electroplating solution turbid and unusable. Even if the electroplating solution is used, the deposited coating is basically a loosely structured byproduct with poor crystallinity, which cannot be used as an anode material for aqueous zinc-ion batteries.
[0100] like Figure 6 The figure shows the chemical composition of the zinc alloy anode (Zn|Sn-1) obtained in Example 1 and the zinc alloy anode (Zn|Sn-2) obtained in Example 2, as determined by inductively coupled plasma atomic emission spectrometry (ICP). Analysis shows that tin metal was successfully deposited into the zinc matrix. Since the concentration of stannous sulfate (SnSO4) in the plating solution of Example 1 was twice that of Example 2, the tin content in the deposited ZnSn alloy anode of Example 1 (Zn|Sn-1) was approximately twice that of Example 2 (Zn|Sn-2), which is consistent with the expected results.
[0101] like Figure 7 As shown, a is the scan image of Example 1 (Zn|Sn-1), b is the scan image of Example 2 (Zn|Sn-2), c is the scan image of Comparative Example 1 (Zn-1), and d is the scan image of Comparative Example 2 (Zn-2). Analysis of the scan images shows that when using a product containing Sn... 2+ During electroplating, zinc metal is deposited onto a copper substrate in a uniform, sheet-like distribution. When Sn is added to the electroplating solution... 2+ At that time, the deposited material exhibited a hexagonal prism morphology. The initial Zn content was... 2+ It is reduced to Zn and uniformly distributed on the copper substrate. Sn is also present. 2+ The reduced deposit is Sn metal, which serves as a nucleation site to guide the growth of Zn spiral dislocations. Finally, the zinc-tin alloy grows into a hexagonal prism morphology. The hexagonal prism morphology is more pronounced in Example 1 (Zn|Sn-1), indicating that when Sn... 2+The higher the concentration, the more pronounced the effect on zinc nucleation and growth.
[0102] like Figure 8 As shown, a) is the cycle performance graph of zinc-symmetric batteries in Example 1 (Zn|Sn-1), Comparative Example 1 (Zn-1), and Comparative Example 3 (Bare Zn). b) is the cycle performance graph of zinc-symmetric batteries in Example 2 (Zn|Sn-2), Comparative Example 2 (Zn-2), and Comparative Example 3 (Bare Zn). In Example 1, the cycle performance was achieved at a current density of 5 mA / cm². –2 Under the condition of 20% anode utilization, the Zn|Sn-1 anode symmetrical cell exhibited a lower initial hysteresis voltage of 50mV and could cycle stably for 2800 hours. After 2800 hours, the hysteresis voltage was only 52mV. The initial hysteresis voltage of the Zn-1 anode was 48mV, but the hysteresis voltage increased significantly with increasing cycle time, and an unavoidable dendrite problem occurred after 500 hours, resulting in a short circuit. In Example 2, at a current density of 5mA / cm²... –2 Under the conditions of 20% anode utilization, the initial hysteresis voltage of the Zn|Sn-2 anode symmetric cell was 55 mV, higher than Zn|Sn-1 but significantly lower than Zn-2 (60 mV). After 700 h, the hysteresis voltage of the Zn|Sn-2 symmetric cell showed a decreasing trend and stabilized for 2000 h, while Zn-2 only stabilized for 580 h before short-circuiting. The initial hysteresis voltage of the pure zinc anode was 89.9 mV, and short-circuiting finally occurred after 220 h. The symmetric cells verified the advantages of the zinc-tin alloy of the present invention in reversible zinc migration: a lower nucleation barrier and faster charge transfer. After cycling for more than 220 h, the voltage curve of the comparative example showed obvious fluctuations, which is a typical feature of violent hydrogen evolution reaction. Its voltage curve approximates a square wave, indicating that a short circuit occurred inside the cell, most likely due to dendrite growth. In contrast, symmetric cells using Zn|Sn alloy electrodes maintained stable voltage curves and showed no significant polarization even after accumulating deposition / stripping for over 2000 hours during prolonged cycling. Furthermore, the depth of discharge (DOD) of the zinc anode is a crucial indicator for evaluating the practical application of zinc-ion batteries, and a high DOD significantly improves the overall energy density of the battery. Even under such demanding testing conditions at a 20% DOD, the Zn|Sn alloy still achieved over 2000 hours of cycling life, almost 10 times that of Bare Zn.
[0103] like Figure 9As shown, a) is the XRD pattern of the negative electrode stripping side of the symmetrical cell (Zn|Sn-1) of Example 1 after 20 cycles, 50 cycles, and 80 cycles; b) is the SEM image of the negative electrode side after 50 cycles; c) is the SEM image of the negative electrode side after 80 cycles. XRD pattern analysis shows that even with a symmetrical cell using a 2M ZnSO4 electrolyte, the Zn|Sn-1 alloy negative electrode maintains a good (002) orientation. Figures b and c show that the columnar structure is maintained after cycling, demonstrating the stability of this structure. The Zn|Sn alloy maintains a flat and dense morphology throughout the deposition / stripping process, indicating that its nucleation and growth processes are more stable.
[0104] like Figure 10 As shown, a) is the full-cell performance graph of Example 1 (Zn|Sn-1) and Comparative Example 3 (Bare Zn), and b) is the full-cell performance graph of Example 2 (Zn|Sn-2) and Comparative Example 3 (Bare Zn). Regarding long-cycle stability, even at 1Ag... -1 At low current densities, the full cell with matched deposited Zn|Sn alloy can still cycle stably for nearly 3000 cycles. However, when bare zinc is used, the full cell only lasts for 500 cycles before its capacity retention drops below 80%. The excellent long-term cycling stability can be attributed to the stable interface on the alloy's negative electrode side. Even after 1000 cycles in the full cell, the Zn|Sn alloy still exhibits a smooth and dense surface morphology. In contrast, bare zinc exhibits uncontrolled zinc deposition / stripping, increasing interfacial impedance and leading to capacity decay.
Claims
1. A method for preparing a zinc alloy negative electrode, characterized in that: Zinc salt, tin salt, complexing agent, and water are mixed to obtain an electroplating solution. Under constant current mode, a zinc-tin binary alloy coating is electrodeposited onto the substrate surface using this solution. The molar ratio of zinc salt to tin salt is 40~20:
1. The complexing agent is EDTA-2Na, and its concentration in the electroplating solution is 0.01~0.1 mol / L. The electrodeposition current density is 5~30 mA / cm². 2 .
2. The preparation method according to claim 1, characterized in that: The zinc salt is ZnSO4·7H2O, ZnCl2 or Zn(CF3SO3)2, and the tin salt is SnSO4 or SnCl2; the concentration of zinc salt in the electroplating solution is 0.1~1 mol / L.
3. The preparation method according to claim 1, characterized in that: The substrate is copper foil, zinc foil, titanium foil, or carbon-based material.
4. The preparation method according to claim 1, characterized in that: The current density of the electrodeposition is 10~20 mA / cm². 2 .
5. The preparation method according to claim 1, characterized in that: The electrodeposition process is as follows: using a zinc sheet as the anode and a copper sheet as the cathode, constant current electrodeposition is performed in an electrolytic cell to deposit a zinc-tin binary alloy plating layer on the copper sheet.
6. The zinc alloy negative electrode prepared by the preparation method according to any one of claims 1-5, characterized in that: The (002) crystal plane of the Zn phase in the zinc alloy negative electrode is the main orientation, and the weight percentage ratio of Zn to Sn is 85~95:5~15.
7. The application of the zinc alloy negative electrode according to claim 6, characterized in that: It was applied to the preparation of aqueous zinc metal batteries.
Citation Information
Patent Citations
Preparation method of zinc molybdate and application of zinc molybdate in lithium ion battery negative electrode material
CN105540669A
Iron-zinc-tin alloy lithium ion battery cathode material
CN106229496A