Bulk acoustic wave filter and method of manufacturing the same
By performing multiple chemical mechanical polishing and ion beam etching polishing processes on the initial electrode layer, a target electrode layer with uniform thickness is formed, and a mass load structure is formed in its edge region. This solves the problem of large bandwidth fluctuations in the bulk acoustic wave filter and improves the device performance.
Patent Information
- Application Number
- CN202210983366.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-16
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-08-16
AI Technical Summary
In the existing technology, the bandwidth of bulk acoustic wave filters fluctuates greatly, mainly due to insufficient uniformity of the lower electrode film, which leads to uneven thickness of the mass load structure and affects device performance.
By performing multiple chemical mechanical polishing and ion beam etching polishing processes on the initial electrode layer, the thickness uniformity of the electrode layer is controlled to form a target electrode layer with uniform thickness, and a mass load structure is formed in its edge region.
This improved the bandwidth stability and device performance of the bulk acoustic wave filter, reduced bandwidth fluctuations, and enhanced the overall performance of the device.
Smart Images

Figure CN117595827B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor device fabrication, specifically to bulk acoustic wave filters and their manufacturing methods. Background Technology
[0002] Bulk acoustic wave filters are widely used in mobile communications. With the development of mobile communications, the performance requirements for bulk acoustic wave filters are getting higher and higher, which also puts forward higher requirements for the manufacturing process of bulk acoustic wave filters.
[0003] The most basic structure of a bulk acoustic wave filter is two metal electrodes sandwiching a piezoelectric thin film. Sound waves oscillate in the piezoelectric thin film to form standing waves. The bandwidth of the bulk acoustic wave filter is controlled by the mass loading structure of the electrodes. In traditional processes, the electrode layer is directly made from the deposited thin film, and then formed into a mass loading structure through other processes to finally obtain the bandwidth we need.
[0004] In traditional processes, the bandwidth of the bulk acoustic wave filter fluctuates significantly, reducing device performance. Summary of the Invention
[0005] In view of this, this application provides a bulk acoustic wave filter and a method for manufacturing the same, which can reduce the bandwidth fluctuation of the bulk acoustic wave filter and improve device performance.
[0006] This application provides a method for manufacturing a bulk acoustic wave filter, comprising the following steps: providing a first substrate wafer, wherein a piezoelectric layer is formed on the surface of the first substrate wafer; forming an initial electrode layer on the surface of the piezoelectric layer, wherein the standard deviation of the thickness of the initial electrode layer in the direction perpendicular to the upper surface of the substrate is a first deviation value; performing a first surface treatment on the initial electrode layer to obtain an intermediate electrode layer; performing an ion beam etching and polishing treatment on the intermediate electrode layer to obtain a target electrode layer, wherein the standard deviation of the thickness of the target electrode layer in the direction perpendicular to the upper surface of the substrate is a second deviation value, the second deviation value being less than the first deviation value; providing a substrate and bonding the target electrode layer to the substrate; removing the first substrate wafer; forming a piezoelectric stack on the substrate, the piezoelectric stack comprising: the target electrode layer, the piezoelectric layer, and an upper electrode layer, wherein the target electrode layer and the upper electrode layer are respectively located on opposite surfaces of the piezoelectric layer; providing a capping wafer and bonding the capping wafer to the surface of the piezoelectric stack opposite to the substrate.
[0007] Optionally, the second deviation value of the target electrode layer is greater than 5% and less than 10%.
[0008] Optionally, the method further includes the step of removing a portion of the target electrode layer to form a mass load structure in the edge region of the target electrode layer.
[0009] Optionally, the first surface treatment includes at least a chemical mechanical polishing (CMP) treatment, and the CMP treatment method includes at least two CMP treatments on the initial electrode layer, wherein the polishing precision of each CMP treatment is progressively increased.
[0010] Optionally, performing two or more chemical mechanical polishing (CMP) treatments on the initial electrode layer includes: performing a first CMP treatment on the initial electrode layer to obtain a first polished layer, the thickness of which is 0.3 to 0.47 times the thickness of the initial electrode layer; and performing a second CMP treatment on the first polished layer to obtain an intermediate electrode layer, the thickness of which is 0.57 to 0.75 times the thickness of the first polished layer, and the thickness of the target electrode layer being 0.84 to 0.96 times the thickness of the intermediate electrode layer.
[0011] Optionally, the particle size of the abrasive particles in the abrasive slurry used in the first chemical mechanical polishing treatment is smaller than the particle size of the abrasive particles in the abrasive slurry used in the second chemical mechanical polishing treatment.
[0012] Optionally, the initial electrode layer is subjected to a first chemical mechanical polishing treatment using a grinding wheel with a rotation speed of 100-110 rpm, the polishing slurry including alumina polishing slurry, a polishing time of 10-15 minutes, and a polishing pressure of 1-1.5 MPa.
[0013] Optionally, a second chemical mechanical polishing treatment is performed on the first polishing layer using a grinding wheel, wherein the grinding wheel rotates at a speed of 70 to 80 rpm, the polishing fluid includes diamond polishing fluid, the polishing time is 5 to 6 minutes, and the polishing pressure is 0.8 to 1 MPa.
[0014] Optionally, during the ion beam etching and polishing process, the radio frequency power range is 55-70W, the ion beam acceleration voltage is 100V-200V, and the ion beam intensity is 3-10mA / cm2.
[0015] Optionally, removing a portion of the target electrode layer to form a mass load structure in the edge region of the target electrode layer includes the following steps: forming a patterned mask layer on the surface of the target electrode layer, the patterned mask layer covering the region where the mass load structure is to be formed; removing a portion of the target electrode layer from the surface of the target electrode layer exposed above the patterned mask layer in a direction perpendicular to the surface of the target electrode layer and downward, and using the target electrode layer covered by the patterned mask layer as the mass load structure, wherein the standard deviation of the thickness of the remaining portion of the exposed surface of the target electrode layer in the direction perpendicular to the upper surface of the substrate is less than the first deviation value.
[0016] Optionally, ion beam etching is performed on the surface of the target electrode layer exposed on the patterned mask layer to remove a portion of the target electrode layer.
[0017] Optionally, the substrate has a cavity structure or a Bragg reflector layer structure.
[0018] Optionally, the method for forming the piezoelectric stack includes: forming an upper electrode layer on the surface of the first substrate wafer; forming a piezoelectric layer on the surface of the upper electrode layer; and forming the initial electrode layer on the piezoelectric layer.
[0019] Optionally, before bonding the substrate to the piezoelectric stack, after removing the first substrate wafer, the target electrode layer is patterned to form the lower electrode.
[0020] Optionally, the method for forming the piezoelectric stack includes: removing the first substrate wafer to expose the piezoelectric layer; forming an upper electrode layer on the piezoelectric layer and patterning the upper electrode layer to form an upper electrode, wherein the upper electrode, the piezoelectric layer, and the target electrode layer constitute a piezoelectric stack.
[0021] This application also provides a bulk acoustic wave filter, which is manufactured by the bulk acoustic wave filter manufacturing method described in any of the above claims.
[0022] In the bulk acoustic wave filter and its manufacturing method in this application, the initial electrode layer undergoes at least a first surface treatment, resulting in a target electrode layer with better uniformity. Furthermore, the surface roughness of the mass load structure formed based on the target electrode layer is reduced, improving the quality of the mass load structure. This helps to improve the bandwidth fluctuation of the bulk acoustic wave filter and enhance device performance. Attached Figure Description
[0023] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0024] Figure 1 This is a schematic flowchart of the steps involved in preparing the target electrode layer in the manufacturing method of the bulk acoustic wave filter described in one embodiment.
[0025] Figures 2 to 6 This is a schematic diagram of the formation process of the target electrode layer in one embodiment.
[0026] Figure 7 This is a schematic diagram of the structure after a mass load structure is formed on the surface of the target electrode layer in one embodiment.
[0027] Figure 8 This is a schematic flowchart of the steps in the bulk acoustic wave filter manufacturing method described in one embodiment.
[0028] Figure 9 This is a schematic diagram of the structure of the bulk acoustic wave filter described in one embodiment. Detailed Implementation
[0029] The inventors discovered that the bandwidth of existing bulk acoustic wave filters fluctuates significantly. Further research revealed that the large bandwidth fluctuation is due to insufficient uniformity of the lower electrode film. The standard deviation of the electrode layer thickness in the direction perpendicular to the upper surface can even reach 50-60 mm, resulting in uneven mass distribution at different locations. Furthermore, forming a load structure directly on the lower electrode film on this basis leads to significant differences in the height of the mass load structure relative to various points on the electrode layer surface. This further contributes to the large bandwidth fluctuation of the filter, reducing device performance.
[0030] To address the aforementioned issues, embodiments of this application provide a bulk acoustic wave filter and its manufacturing method to resolve the problem of poor uniformity of the lower electrode thin film, thereby optimizing the bandwidth fluctuation of the bulk acoustic wave filter and improving device performance.
[0031] The sensor packaging structure and packaging method of the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. The advantages and features of the present invention will become clearer from the following description and drawings; however, it should be noted that the concept of the technical solution of the present invention can be implemented in many different forms and is not limited to the specific embodiments described herein. The accompanying drawings are all in a very simplified form and use non-precise proportions, and are only used to facilitate and clarify the illustration of the embodiments of the present invention.
[0032] The terms “first,” “second,” etc., used in the specification and claims are used to distinguish between similar elements and are not necessarily used to describe a particular order or chronological sequence. It should be understood that these terms, used so in this way, may be replaced where appropriate, for example, to allow embodiments of the invention described herein to operate in a different order than that described or shown herein. Similarly, if the methods described herein comprise a series of steps, and the order of these steps presented herein is not necessarily the only possible order in which these steps can be performed, and some described steps may be omitted and / or some other steps not described herein may be added to the method. If a component in one figure is identical to a component in another figure, although these components are readily identifiable in all figures, this specification will not label all identical components in every figure for the sake of clarity.
[0033] This application provides a method for fabricating a target electrode layer in the fabrication process of a bulk acoustic wave filter.
[0034] Please see Figures 1 to 6 , Figure 1 This is a schematic flowchart of the steps involved in preparing the target electrode layer in one embodiment. Figures 2 to 6 This is a schematic diagram of the process of forming the target electrode layer in one embodiment.
[0035] In this embodiment, the method for preparing the target electrode layer includes the following steps:
[0036] Step S1: Provide substrate 101;
[0037] Step S2: An initial electrode layer 102 is formed on the upper surface of the substrate 101, and the standard deviation of the thickness of the initial electrode layer in the direction perpendicular to the upper surface of the substrate 101 is a first deviation value.
[0038] Step S3: Perform a first surface treatment on the initial electrode layer 102 to obtain the intermediate electrode layer 1022;
[0039] Step S4: Perform ion beam etching and polishing on the intermediate electrode layer 1022 to obtain the target electrode layer 1023, and the standard deviation of the thickness of the target electrode layer 1023 in the direction perpendicular to the upper surface of the substrate is the second deviation value, which is less than the first deviation value.
[0040] Please see Figure 2 This is a schematic diagram of the structure of the substrate 101 in one embodiment.
[0041] In some embodiments, the substrate 101 is made of semiconductor materials, such as silicon (Si), germanium (Ge), silicon germanium (SiGe), silicon carbide (SiC), silicon carbide (SiGeC), indium arsenide (InAs), gallium arsenide (GaAs), indium phosphide (InP), or other III / V compound semiconductors. It can also be a double-sided polished wafer (DSP), or a ceramic substrate such as alumina, a quartz substrate, or a glass substrate. Other material layers, such as a piezoelectric layer, are formed on the substrate 101 prior to the formation of the target electrode layer.
[0042] Those skilled in the art can also select the specific material of the substrate 101 as needed.
[0043] Please see Figure 3 This is a schematic diagram of the structure after the piezoelectric structure 200 is formed on the substrate 101.
[0044] exist Figure 3In the illustrated embodiment, the piezoelectric structure 200 further includes a piezoelectric layer 103 located above the substrate 101. The initial electrode layer 102 is located on the upper surface of the piezoelectric layer 103, and the piezoelectric structure 200 further includes an upper electrode layer 104 located between the piezoelectric layer 103 and the substrate 101.
[0045] Both the upper electrode layer 104 and the initial electrode layer 102 can be used as input or output electrodes for receiving or providing electrical signals such as radio frequency (RF) signals. The upper electrode layer 104 can be used to prepare the input electrode and the initial electrode layer 102 to prepare the output electrode, or vice versa. The piezoelectric layer 103 can convert electrical signals input through the upper electrode layer 104 or the initial electrode layer 102 into bulk sound waves. For example, the piezoelectric layer 103 converts electrical signals into bulk sound waves through physical vibration.
[0046] In some embodiments, the materials of the upper electrode layer 104 and the initial electrode layer 102 can be metallic materials with conductive properties, such as those made from one of the following metals: molybdenum (Mo), aluminum (Al), copper (Cu), tungsten (W), tantalum (Ta), platinum (Pt), ruthenium (Ru), rhodium (Rh), iridium (Ir), chromium (Cr), titanium (Ti), gold (Au), osmium (Os), rhenium (Re), palladium (Pd), or a stack formed of the above metals.
[0047] In some embodiments, the initial electrode layer 102 comprises a molybdenum layer with a thickness greater than or equal to [a certain value]. For example The initial electrode layer 102 is formed on the upper surface of the piezoelectric layer using at least one of physical vapor deposition, chemical vapor deposition, and atomic layer deposition.
[0048] In some embodiments, the upper electrode layer 104 and the initial electrode layer 102 can be formed by physical vapor deposition or chemical vapor deposition methods such as magnetron sputtering or evaporation.
[0049] In some embodiments, the piezoelectric layer 103 may be deposited using chemical vapor deposition, physical vapor deposition, or atomic layer deposition.
[0050] In some embodiments, the piezoelectric layer 103 may be made of piezoelectric materials with a wurtzite-type crystalline structure, such as aluminum nitride (AlN), zinc oxide (ZnO), lead zirconate titanate (PZT), lithium niobate (LiNbO3), quartz, potassium niobate (KNbO3), or lithium tantalate (LiTaO3), or combinations thereof. When the piezoelectric layer 103 comprises aluminum nitride (AlN), it may also comprise at least one rare earth metal, such as scandium (Sc), erbium (Er), yttrium (Y), and lanthanum (La). Furthermore, when the piezoelectric layer 103 comprises aluminum nitride (AlN), it may also comprise at least one transition metal, such as zirconium (Zr), titanium (Ti), manganese (Mn), and hafnium (Hf).
[0051] exist Figure 3 In the embodiment shown, the thickness of the initial electrode layer 102 is h1. Due to the preparation method used, the surface has certain undulations. Therefore, the standard deviation of the thickness of the initial electrode layer 102 in the direction perpendicular to the upper surface of the substrate 101 is the first deviation value, which is usually greater than 12% and generally between 50% and 60%.
[0052] In some embodiments, the film layer prepared by common preparation methods can be directly used as the initial electrode layer 102, thereby reducing the control precision requirements of these preparation methods. Common film preparation methods do not have sufficient control precision to directly prepare a material layer with the required flatness. Therefore, the uniformity of the film thickness of the initial electrode layer 102 is poor, and the standard deviation of the thickness is a first deviation value.
[0053] In this embodiment, please refer to 4 to Figure 5 The initial electrode layer 102 is subjected to a first surface treatment to form an intermediate electrode layer 1022.
[0054] In some embodiments, the first surface treatment includes at least a chemical mechanical polishing (CMP) process, wherein the CMP process includes at least two CMP processes on the initial electrode layer, with the polishing precision increasing progressively in each CMP process. The first surface treatment employs a faster CMP method, which can accelerate the surface treatment speed.
[0055] Ion beam etching can achieve more accurate planarization results. Therefore, in some embodiments, ion beam etching can be used as the final surface treatment process, and ion beam etching can also be introduced in the first surface treatment process.
[0056] In some embodiments, using the surface treatment method described in this embodiment, a target electrode layer 1023 with a thickness close to the target thickness can be effectively obtained by ion beam etching at the end. In some embodiments, the thickness of the initial electrode layer 102 is greater than or equal to a first preset thickness, and the thickness of the target electrode layer 1023 is a second preset thickness, which is less than the first preset thickness.
[0057] In this embodiment, the first surface treatment of the initial electrode layer 102 includes two chemical mechanical polishing processes, specifically including: performing a first chemical mechanical polishing process on the initial electrode layer 102 to obtain a first polished layer 1021 (please refer to...). Figure 4 The first polishing layer 1021 is subjected to a second chemical mechanical polishing treatment to obtain the intermediate electrode layer 1022 (see reference). Figure 5 The polishing precision of the first chemical mechanical polishing treatment is less than that of the second chemical mechanical polishing treatment.
[0058] Please see Figure 4 This is a schematic diagram of the structure of the initial electrode layer 102 after undergoing a first chemical mechanical polishing treatment in one embodiment.
[0059] In this embodiment, the initial electrode layer 102 is thinned after being subjected to a first chemical mechanical polishing treatment to obtain a first polished layer 1021. The thickness of the first polished layer 1021 is h2. After the surface is subjected to the first chemical mechanical polishing treatment, the degree of undulation is reduced. Therefore, the standard deviation of the thickness of the first polished layer 1021 in the direction perpendicular to the upper surface of the substrate 101 is close to a preset value.
[0060] Please see Figure 5 This is a schematic diagram of the structure of the initial electrode layer 102 after a second chemical mechanical polishing treatment in one embodiment.
[0061] In this embodiment, the first polishing layer 1021 is further thinned to obtain an intermediate electrode layer 1022 with a thickness of h3. The surface of the intermediate electrode layer 1022 is subjected to a second chemical mechanical polishing treatment, which further reduces the degree of undulation. Therefore, the standard deviation of the thickness of the intermediate electrode layer 1022 in the direction perpendicular to the upper surface of the substrate 101 is further close to the preset value.
[0062] The first chemical mechanical polishing (CMP) process corresponds to coarse polishing, and the second CMP process corresponds to fine polishing. Coarse polishing can achieve rapid thinning of the initial electrode layer 102, shortening the time spent in the entire polishing process. The standard deviation of the thickness of the resulting first polished layer 1021 is less than the first deviation value, but does not meet the second deviation value requirement. Fine polishing can further optimize the standard deviation of the thickness of the intermediate electrode layer obtained based on coarse polishing, further approaching the second deviation value requirement.
[0063] In some embodiments, the thickness of the first polishing layer is 0.3 to 0.47 times the thickness of the initial electrode layer, the thickness of the intermediate electrode layer is 0.57 to 0.75 times the thickness of the first polishing layer, and the thickness of the target electrode layer is 0.84 to 0.96 times the thickness of the intermediate electrode layer.
[0064] In some embodiments, the particle size of the abrasive particles in the polishing slurry used in the first chemical mechanical polishing (CMP) treatment is smaller than that of the abrasive particles in the polishing slurry used in the second CMP treatment. Generally, an alumina polishing slurry can be used in the first CMP treatment, and a diamond polishing slurry can be used in the second CMP treatment. The particle sizes of the abrasive particles in these two slurries meet the requirements. Specifically, the particle size of the alumina polishing slurry is between 50 nm and 200 nm, and the particle size of the diamond polishing slurry is between 5 nm and 100 nm.
[0065] Furthermore, the alumina polishing slurry has an excellent removal rate for hard substrates, sapphire substrates, etc., and can quickly rough grind the surface of the initial electrode layer without forming other structures, thereby accelerating the overall polishing speed.
[0066] In some embodiments, the thickness of the initial electrode layer is to The thickness of the first polishing layer 1021 is to The thickness of the intermediate electrode layer 1022 is to The thickness of the target electrode layer 1023 is to
[0067] In some embodiments, the initial electrode layer 102 is subjected to a first chemical mechanical polishing treatment using a grinding wheel at a rotation speed of 100-110 rpm, the polishing slurry comprising alumina polishing slurry, the polishing time being 10-15 minutes, and the polishing pressure being 1-1.5 MPa, thereby obtaining a layer with a thickness of 6000 nm. The first polished layer 1021.
[0068] In some embodiments, the first polished layer 1021 is subjected to a second chemical mechanical polishing treatment using a grinding wheel, wherein the grinding wheel rotates at a speed of 70-80 rpm, the polishing slurry includes diamond polishing slurry, the polishing time is 5-6 minutes, and the polishing pressure is 0.8-1 MPa, thereby obtaining a layer with a thickness of 4000 mm. The intermediate electrode layer 1022.
[0069] The first chemical mechanical polishing (CMP) process is a coarse grinding process, which requires removing a relatively thick initial electrode layer. Therefore, the grinding time is long, the grinding pressure is high, and the grinding speed is fast. The second CMP process is a fine grinding process. In this case, the standard deviation of the thickness of the first polished layer is smaller than the standard deviation of the thickness of the initial electrode layer. Therefore, the thickness of the first polished layer to be removed is thinner, the grinding time is short, the grinding pressure is low, and the grinding speed is slow.
[0070] Using two chemical mechanical polishing processes can effectively control the thickness of the initial electrode layer that is removed by grinding, preventing the removal of too much initial electrode layer due to only coarse grinding. It can also effectively control the time required to grind to the target electrode layer, preventing the time spent grinding to the target electrode layer due to only fine grinding.
[0071] Please refer to Figure 6 The intermediate electrode layer 1022 is subjected to ion beam etching and polishing to obtain the target electrode layer 1023, and the final target electrode layer 1023 has better uniformity.
[0072] The radio frequency power range used in the ion beam etching and polishing process is 55–70W, the ion beam acceleration voltage is 100V–200V, and the ion beam intensity is 3–10mA / cm. 2 .
[0073] In some embodiments, an ion beam etching and polishing process is performed using an ion beam apparatus. The apparatus parameters include: RF power of the ion beam source of 63 to 66 W, beam voltage of 1305 to 1310 V, ion current of 8 to 11 mA, and accelerating voltage of 145 to 153 V; neutralizer emission current of 26 to 32 mA; and ion beam intensity of 5 to 6 mA / cm². 2Under these machine parameters, the ions provided by the ion beam machine can meet the above-mentioned current density requirements, ion energy requirements, and etching angle requirements.
[0074] Based on the above-mentioned equipment parameters, the current density of the ion beam, the ion energy, and the angle range of the ion beam etching the target film can be within the required range.
[0075] In some embodiments, at least one of overall bombardment, partitioned bombardment, or point-by-point bombardment can be used to etch the intermediate electrode layer 1022 using an ion beam (see reference). Figure 5 This allows the surface of the intermediate electrode layer 1022 to be partially etched to a predetermined thickness, ultimately achieving the thickness requirement of the target electrode layer 1023 and improving the uniformity of the target electrode layer's thickness.
[0076] In fact, the area of a single ion beam bombardment is related to the size of the target electrode layer, so the area of a single ion beam bombardment can be selected as needed.
[0077] Figure 6 In the process, the intermediate electrode layer 1022 is further thinned to obtain the target electrode layer 1023, which has a thickness of h4. The surface of the target electrode layer 1023 is etched by an ion beam, and the standard deviation of the thickness in the direction perpendicular to the upper surface of the substrate 101 meets the second deviation value requirement.
[0078] Research has found that when the second deviation value of the target electrode layer 1023 is within 5 to 10, the thickness uniformity of the target electrode layer 1023 is good, and the mass loading structure 201 formed based on the target electrode layer 1023 also has good uniformity. The bandwidth fluctuation range of the thin-film bulk acoustic filter formed based on this semiconductor device is small, and the device performance is optimized. Therefore, in some embodiments, the second deviation value of the target electrode layer is greater than 5% and less than 10%.
[0079] In some preferred embodiments, the second deviation value is in the range of 2% to 3%, thereby achieving the best device optimization effect.
[0080] In some embodiments, the upper surface of the target electrode layer 1023 may further include a passivation layer, which covers the initial electrode layer 102. The passivation layer may be made of silicon dioxide (SiO2), silicon nitride (Si3N4), silicon oxynitride (SiON), aluminum nitride (AlN), aluminum oxide (Al2O3), etc.
[0081] In some other embodiments, the initial electrode layer can be processed into the target electrode layer by ion beam etching alone. That is, the first surface treatment also adopts the ion beam etching process, which is suitable for cases where the initial electrode layer is thin and the thickness standard deviation is small, thereby reducing the waste of energy in ion beam etching while taking into account the processing accuracy.
[0082] Please refer to Figure 7 In this embodiment, the method further includes the step of removing a portion of the target electrode layer 1023 to form a mass load structure 201 in the edge region of the target electrode layer 1023.
[0083] When the mass load structure 201 is formed based on the target electrode layer 1023, the surface roughness of the final mass load structure 201 is reduced, which can effectively improve the quality of the mass load structure 201, thereby helping to improve the bandwidth fluctuation of the bulk acoustic wave filter and enhance the device performance.
[0084] exist Figure 7 In the illustrated embodiment, removing a portion of the target electrode layer 1023 to form a mass load structure in the edge region of the target electrode layer includes the following steps: forming a patterned mask layer on the surface of the target electrode layer 1023, the patterned mask layer covering the area where the mass load structure 201 is to be formed; removing a portion of the target electrode layer from the surface of the target electrode layer exposed above the patterned mask layer in a direction perpendicular to the surface of the target electrode layer downwards, and using the target electrode layer covered by the patterned mask layer as the mass load structure, wherein the standard deviation of the thickness of the remaining portion of the exposed surface of the target electrode layer in the direction perpendicular to the upper surface of the substrate is less than the first deviation value.
[0085] In some embodiments, ion beam etching is performed on the surface of the target electrode layer exposed on the patterned mask layer to remove a portion of the target electrode layer.
[0086] In this embodiment, the thickness of the removed portion of the target electrode layer is on the order of 10 nanometers. It is difficult to achieve such thinning precision using conventional polishing processes. Therefore, ion beam etching, which can meet the process requirements, is used to partially remove the target electrode layer to achieve the required processing precision.
[0087] In some embodiments, the mask layer is a photomask layer, and the photomask layer can be patterned by performing an exposure process on the photomask layer.
[0088] In some embodiments, the top surface of the mass load structure 201 and the top surface of the target electrode layer 1023 in the region after the removal of the portion have a height difference, which can be set according to actual usage requirements. The width of the mass load structure 201 can be set according to actual usage requirements.
[0089] In some embodiments, the mass load structure 201 is in the form of a rectangular ring, surrounding the central region of the piezoelectric structure 200 and along the periphery of the substrate 101. In practice, the specific shape of the mass load structure 201 can also be configured as needed.
[0090] In a second aspect, this application also provides a method for manufacturing a bulk acoustic wave filter.
[0091] Please see Figure 8 This is a schematic flowchart illustrating the steps of a bulk acoustic wave filter manufacturing method described in one embodiment. (See also reference...) Figure 9 This is a schematic diagram of the structure of the formed bulk acoustic wave filter.
[0092] The bulk acoustic wave filter manufacturing method includes the following steps:
[0093] Step S101: Provide a first substrate wafer, on which a piezoelectric layer is formed.
[0094] In this embodiment, only a piezoelectric layer 805 is formed on the first substrate wafer.
[0095] In other embodiments, an upper electrode layer is formed on the surface of the first substrate wafer; and then the piezoelectric layer 805 is formed on the surface of the upper electrode layer.
[0096] Step S102: An initial electrode layer is formed on the surface of the piezoelectric layer, and the standard deviation of the thickness of the initial electrode layer in the direction perpendicular to the upper surface of the substrate is a first deviation value.
[0097] Step S103: Perform a first surface treatment on the initial electrode layer to obtain an intermediate electrode layer.
[0098] Step S104: Perform ion beam etching and polishing on the intermediate electrode layer to obtain the target electrode layer, and the standard deviation of the thickness of the target electrode layer in the direction perpendicular to the upper surface of the substrate is the second deviation value, which is less than the first deviation value.
[0099] The above steps form a target electrode layer of uniform thickness on the surface of the piezoelectric layer. A load structure can also be formed on the target electrode layer.
[0100] Step S105: Provide a substrate and bond the target electrode layer to the substrate.
[0101] In this embodiment, before bonding the substrate, the target electrode layer can be patterned to form a lower electrode 807, and then the substrate 801 can be bonded to the lower electrode 807.
[0102] Step S106: Remove the first substrate wafer and form a piezoelectric stack on the substrate. The piezoelectric stack includes the target electrode layer, the piezoelectric layer and the upper electrode layer, with the target electrode layer and the upper electrode layer located on opposite surfaces of the piezoelectric layer.
[0103] In this embodiment, after removing the first substrate wafer, the other side surface of the piezoelectric layer 805 is exposed. Then, after forming an upper electrode layer on the other side surface of the piezoelectric layer 805, the upper electrode layer is patterned to form an upper electrode 806, thereby forming the piezoelectric stack.
[0104] In other embodiments, in step S101, a lower electrode layer and a piezoelectric layer may be formed on the surface of the first substrate wafer. After the first substrate wafer is removed, the lower electrode layer is directly exposed. After the lower electrode layer is patterned, a lower electrode is formed.
[0105] Step S107: Provide a capping wafer and bond the capping wafer to the surface of the piezoelectric stack opposite to the substrate.
[0106] In this embodiment, the capping wafer 801 is bonded to one side of the upper electrode 806 and is opposite to the upper electrode 806.
[0107] The relevant features in this embodiment are consistent with those described in the previous embodiments, and will not be repeated here. The bulk acoustic wave filter formed by the above method has a uniform lower electrode thickness, which can optimize the quality of the mass load structure finally formed on the lower electrode, help reduce the bandwidth fluctuation of the finally formed bulk acoustic wave filter, and improve the device performance.
[0108] Please see Figure 9 This is a schematic diagram of the structure of a bulk acoustic wave filter formed in one embodiment of the present invention.
[0109] In this embodiment, the bulk acoustic wave filter is manufactured using the aforementioned bulk acoustic wave filter manufacturing method. In this embodiment, the surface of the lower electrode 807 is coated with a TEOS film layer 809.
[0110] In this embodiment, the substrate 801 has a cavity structure or a Bragg reflector layer structure within the bonding layer, and a cavity 804 is also formed between the substrate 801 and the piezoelectric stack. Furthermore, a deep via 803 is formed within the substrate 801 to expose the lower electrode 807. The substrate 801 also contains some functional structures, including a SiN film, etc., which are not shown in the figure.
[0111] In some embodiments, the deep through-hole 803 may be filled with a conductive plug, the bottom of which is electrically connected to the lower electrode 807, and the top of which has a conductive contact point protruding from the surface of the substrate 801, such as a solder ball or a conductive protrusion. The conductive contact point is electrically connected to the lower electrode 807 through the conductive plug, serving as an interconnection structure for electrical connection with external structures, thereby electrically leading out the lower electrode 807.
[0112] In some embodiments, the Bragg reflector structure comprises at least two layers of optical material and is an adjustable multilayer structure. The thickness of each layer of the Bragg reflector structure corresponds to a quarter of the wavelength and can be used to reflect signals.
[0113] In this embodiment, two metal bonds are also provided on the side of the piezoelectric stack. The metal bonds include at least a Ti layer 810 and a Cu layer 808, which are arranged sequentially. The Ti layer 810 is located on the side of the piezoelectric stack, and the Cu layer 808 is located on the outer surface of the Ti layer.
[0114] In this embodiment, a capping wafer 802 is also disposed below the piezoelectric stack. The capping wafer 802 is bonded to one side of the upper electrode 806 by bonding bonds or support pillar structures, and is opposite to the upper electrode 806, thereby realizing the encapsulation of the bulk acoustic wave filter.
[0115] In this embodiment, the bulk acoustic wave filter has an electrode layer with better uniformity and a mass load structure with higher quality, which helps to reduce bandwidth fluctuations and improve device performance.
[0116] It should be noted that the various embodiments in this specification are described in a related manner, and the same or similar parts between the various embodiments can be referred to mutually. Each embodiment focuses on describing the differences from other embodiments. In particular, for structural embodiments, since they are basically similar to method embodiments, the description is relatively simple, and the relevant parts can be referred to the description of the method embodiments.
[0117] The above description is merely an embodiment of this application and does not limit the patent scope of this application. Any equivalent structural or procedural transformations made using the content of this application's specification and drawings, such as the combination of technical features between embodiments, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of this application.
Claims
1. A method of manufacturing a bulk acoustic wave filter, characterized by, The method comprises the following steps: providing a first substrate wafer, a piezoelectric layer being formed on a surface of the first substrate wafer; forming an initial electrode layer on the surface of the piezoelectric layer, a standard deviation of thickness of the initial electrode layer in a direction perpendicular to the upper surface of the substrate being a first deviation value; performing a first surface treatment on the initial electrode layer to obtain an intermediate electrode layer, the first surface treatment comprising at least a chemical mechanical polishing treatment, the chemical mechanical polishing treatment comprising at least two or more chemical mechanical polishing treatments, and polishing accuracy of different chemical mechanical polishing treatments being improved gradually; performing ion beam etching and polishing treatment on the intermediate electrode layer to obtain a target electrode layer, a standard deviation of thickness of the target electrode layer in a direction perpendicular to the upper surface of the substrate being a second deviation value, the second deviation value being smaller than the first deviation value; bonding the target electrode layer to a base; removing the first substrate wafer to form a piezoelectric stack on the base, the piezoelectric stack comprising the target electrode layer, the piezoelectric layer and an upper electrode layer, the target electrode layer and the upper electrode layer being respectively located on opposite surfaces of the piezoelectric layer; bonding a cover wafer to a surface of the piezoelectric stack opposite to the base.
2. The production method according to claim 1, characterized by The second deviation value of the target electrode layer is greater than 5% and smaller than 10%.
3. The production method according to claim 1, characterized by The method further comprises the following steps: removing part of the target electrode layer to form a mass load structure in an edge region of the target electrode layer.
4. The production method according to claim 1, characterized by The two or more chemical mechanical polishing treatments on the initial electrode layer comprise: performing a first chemical mechanical polishing treatment on the initial electrode layer to obtain a first polishing layer, a thickness of the first polishing layer being 0.3 to 0.47 times a thickness of the initial electrode layer; performing a second chemical mechanical polishing treatment on the first polishing layer to obtain the intermediate electrode layer, a thickness of the intermediate electrode layer being 0.57 to 0.75 times the thickness of the first polishing layer, and a thickness of the target electrode layer being 0.84 to 0.96 times the thickness of the intermediate electrode layer.
5. The production method according to claim 4, characterized by Grinding particles in a polishing liquid used in the first chemical mechanical polishing treatment have a particle size smaller than that of grinding particles in a polishing liquid used in the second chemical mechanical polishing treatment.
6. The production method according to claim 5, wherein The first chemical mechanical polishing treatment on the initial electrode layer is performed using a grinding wheel, a rotation speed of the grinding wheel being 100 to 110 revolutions per minute, the polishing liquid comprising an alumina polishing liquid, a polishing time being 10 to 15 minutes, and a polishing pressure being 1 to 1.5 MPa.
7. The production method according to claim 6, wherein The second chemical mechanical polishing treatment on the first polishing layer is performed using a grinding wheel, a rotation speed of the grinding wheel being 70 to 80 revolutions per minute, the polishing liquid comprising a diamond polishing liquid, a polishing time being 5 to 6 minutes, and a polishing pressure being 0.8 to 1 MPa.
8. The production method according to claim 1, characterized by The ion beam etching polishing treatment is performed at a radio frequency power of 55-70 W, an ion beam acceleration voltage of 100-200 V, and an ion beam intensity of 3-10 mA / cm 2 .
9. The production method according to claim 3, wherein The removing part of the target electrode layer to form the mass load structure in the edge region of the target electrode layer comprises the following steps: forming a patterned mask layer on the surface of the target electrode layer, the patterned mask layer covering an area where the mass load structure is to be formed; Part of the target electrode layer is removed along a direction perpendicular to the surface of the target electrode layer and exposed to the surface of the patterned mask layer, and the target electrode layer under the patterned mask layer is used as the mass loading structure, and the standard deviation of the thickness of the remaining part of the surface of the target electrode layer exposed to the surface of the patterned mask layer in the direction perpendicular to the surface of the substrate is less than the first deviation value.
10. The manufacturing method according to claim 9, wherein The surface of the target electrode layer exposed to the surface of the patterned mask layer is subjected to ion beam etching to remove part of the target electrode layer.
11. The method of manufacturing a bulk acoustic wave filter according to claim 1, wherein, The substrate has a cavity structure or a Bragg reflection layer structure.
12. The method of claim 1, wherein The method for forming the piezoelectric stack includes: forming an upper electrode layer on the surface of the first substrate wafer; forming a piezoelectric layer on the surface of the upper electrode layer; and forming the initial electrode layer on the piezoelectric layer.
13. The method of manufacturing a bulk acoustic wave filter according to claim 12, wherein, Before the substrate is bonded to the piezoelectric stack, the target electrode layer is patterned to form a lower electrode after the first substrate wafer is removed.
14. The method of manufacturing a bulk acoustic wave filter according to claim 1, wherein, The method for forming the piezoelectric stack includes: removing the first substrate wafer to expose the piezoelectric layer. An upper electrode layer is formed on the piezoelectric layer, and the upper electrode layer is patterned to form an upper electrode, and the upper electrode, the piezoelectric layer, and the target electrode layer constitute a piezoelectric stack.
15. A bulk acoustic wave filter, comprising: The bulk acoustic wave filter is manufactured by the method of any one of claims 1 to 14.
Citation Information
Patent Citations
Single-crystal piezoelectric thin film-based sound wave resonator and fabrication method thereof
CN108493326A
Monocrystal FBAR piezoelectric film and preparation method thereof
CN114362704A