A loading rate based pre-strengthening forming method for 7xxx series aluminum alloys
By optimizing the aluminum alloy forming process parameters through a pre-strengthening forming method based on loading rate, the influence of mold loading method and loading rate on forming effect was resolved, thereby improving the performance and production applicability of aluminum alloy components.
Patent Information
- Application Number
- CN202311487267.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-07
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-07
AI Technical Summary
Existing aluminum alloy forming processes do not fully consider the impact of mold loading methods and loading rates on forming results, resulting in inconsistent performance of formed components.
A method for pre-strengthening and forming 7xxx series aluminum alloys based on loading rate is provided. By obtaining W-state aluminum alloy billets for pre-strengthening treatment, and combining heating and holding time with the loading rate of forming mold, the heating temperature and holding time are determined to match different mold loading methods and loading rates, thereby optimizing the forming process parameters.
It has been achieved that high-performance aluminum alloy formed components can be obtained under different mold loading methods and loading rates, which improves the mechanical properties and production applicability of the formed components and simplifies the production process.
Smart Images

Figure CN117600264B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloy processing technology, and in particular to a pre-strengthening forming method for 7xxx series aluminum alloys based on loading rate. Background Technology
[0002] In recent years, to address the poor room-temperature plasticity of aluminum alloys, especially 7xxx series aluminum alloys, the method of heating aluminum alloys to high temperatures for forming has been increasingly used. Depending on the forming temperature, with the recrystallization temperature as the boundary, high-temperature forming of aluminum alloys is divided into two methods: hot forming and warm forming. Currently, the hot forming process for aluminum alloys is based on the integrated hot forming-quenching process developed by Professor Lin Jianguo of Imperial College London. This process, the most widely used, combines hot forming and heat treatment of aluminum alloys. After solution treatment, the aluminum alloy sheet is rapidly transferred to a water-cooled mold and quickly closed to form the shape. After forming, the mold is held closed for pressure quenching, and finally, aging treatment is performed to improve strength. This process effectively solves the problem of poor precision in traditional hot forming processes. However, due to its long production cycle and high energy consumption, it is not suitable for... Process improvements are also ongoing, such as the introduction of methods like rapid solution treatment and rapid aging.
[0003] In recent years, the warm forming process of 7xxx series high-strength aluminum alloys has also come into focus. To avoid the subsequent artificial aging step, most 7xxx series alloys in the peak-aged state (T6 state) are used as billets for warm forming, with the forming temperature typically controlled below 250℃. However, once the T6 state alloy is heated to a high temperature, its precipitated phases inevitably coarsen, and at excessively high temperatures, they may even transform into non-strengthening phases, significantly reducing the material strength. If the influence on the precipitated phases is reduced by lowering the temperature, the improvement in the plasticity of the T6 state alloy is limited.
[0004] Patent document CN112264498A discloses a method for hot stamping forming of aluminum alloys with reinforcement. First, different series of aluminum alloys are pre-strengthened to obtain GP zones. Then, the sheet metal is heated to different temperature ranges for holding and hot stamping to obtain the final component. However, in actual industrial production, aluminum alloys are widely used, resulting in a wide variety of formed parts, and correspondingly, various forming methods. The production cycle of forming dies for different parts and different forming processes may vary greatly, and the loading methods and loading rates of the forming dies also differ significantly. This necessitates that the forming process and the die loading method be adapted to obtain parts with ideal performance.
[0005] Current forming processes rarely consider the impact of mold loading methods and rates on the forming results. However, different loading methods correspond to different loading rates, leading to different microstructural evolutions in the material during forming, especially for warm forming. Existing forming processes ignore the influence of mold loading methods and rates on the forming results, applying the same pretreatment process to different mold loading methods and rates. This results in inconsistent performance of the final formed components. Summary of the Invention
[0006] In view of this, it is necessary to provide a pre-strengthening forming method for 7xxx series aluminum alloys based on loading rate, which can determine the relevant parameters of the pretreatment process according to the mold loading method and loading rate, so as to obtain forming components with ideal performance under various mold loading methods and loading rates.
[0007] To achieve the above objectives, the present invention provides a method for pre-strengthening forming of 7xxx series aluminum alloys based on loading rate, comprising the following steps:
[0008] S1. Obtain W-state 7xxx series aluminum alloy billet, and perform pre-strengthening treatment on the W-state 7xxx series aluminum alloy billet to obtain pre-strengthened aluminum alloy billet;
[0009] S2. The pre-strengthened aluminum alloy billet is heated and held at a certain temperature, wherein the holding time is determined according to the heating temperature and the loading rate of the forming mold used subsequently.
[0010] S3. The heated and heat-insulated aluminum alloy billet is shaped using a forming mold to obtain the final component. The temperature of the forming mold is determined by the loading rate of the forming mold.
[0011] In some embodiments, in step S1, the temperature of the pre-strengthening treatment of the W-state 7xxx series aluminum alloy billet to obtain the pre-strengthened aluminum alloy billet is 50-150℃, and the time of the pre-strengthening treatment is 1-24h.
[0012] In some embodiments,
[0013] In step S2, the holding time is determined based on the heating temperature and the loading rate of the forming mold used subsequently, specifically as follows:
[0014] (1) If the loading rate of the forming die is 0.1-10s -1 When the heating temperature of the pre-strengthened aluminum alloy billet is 150-200℃, the holding time is 5-30 minutes; when the heating temperature of the pre-strengthened aluminum alloy billet is 200-250℃, the holding time is 1-20 minutes.
[0015] (2) If the loading rate of the forming die is 0.001-0.1s -1 When the heating temperature of the pre-strengthened aluminum alloy billet is 150-200℃, the holding time is 3-20 minutes; when the heating temperature of the pre-strengthened aluminum alloy billet is 200-250℃, the holding time is 0-15 minutes.
[0016] (3) If the loading rate of the forming die is less than 0.001s -1 When the heating temperature of the pre-strengthened aluminum alloy billet is 150-200℃, the holding time is 1-15 minutes; when the heating temperature of the pre-strengthened aluminum alloy billet is 200-250℃, the holding time is 0-10 minutes.
[0017] In some embodiments, if an air furnace is used for heating, the greater the thickness of the pre-strengthened aluminum alloy billet, the longer the heating time is required.
[0018] In some embodiments, if the final component after molding needs to undergo a subsequent paint baking process, the heat preservation time in step S2 should be shortened.
[0019] In some embodiments, in step S3, the temperature of the forming mold is determined by the loading rate of the forming mold, specifically:
[0020] If the loading rate of the forming die is between 0.005 and 10 s -1 In this case, the forming mold can be a cold mold or a warm mold;
[0021] If the loading rate of the forming die is less than 0.005s -1 If so, a warm mold is used for forming.
[0022] In some embodiments, the mold temperature of the warm mold is not higher than the heating temperature in step S2.
[0023] In some embodiments, the mold temperature of the warm mold is 0-50°C lower than the heating temperature in step S2.
[0024] In some embodiments, the method for obtaining the W-state 7xxx series aluminum alloy billet in step S1 is to perform a solution treatment on the aluminum alloy billet to obtain the W-state 7xxx series aluminum alloy billet.
[0025] In some embodiments, in step S3, the loading rate of the forming mold is constant or variable.
[0026] Compared with the prior art, the beneficial effects of the technical solution proposed in this invention are: the forming process disclosed in this invention fully considers the loading rate of different parts and different forming methods as well as the equipment conditions of the forming mold, and customizes the process parameters of heating and heat preservation and molding, so that the heating temperature and heat preservation time are matched with the subsequent forming loading rate, thereby enabling the final aluminum alloy component to achieve the best performance. Attached Figure Description
[0027] Figure 1 This is a schematic flowchart of an embodiment of the pre-strengthening forming method for 7xxx series aluminum alloys based on loading rate provided by the present invention;
[0028] Figure 2 This is a schematic diagram illustrating the changes in temperature and microstructure of aluminum alloy billets during the forming process provided by the present invention. Detailed Implementation
[0029] Preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which form part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.
[0030] Please refer to Figure 1 This invention provides a method for pre-strengthening and forming 7xxx series aluminum alloys based on loading rate, comprising the following steps:
[0031] S1. Obtain W-state 7xxx series aluminum alloy billet, and perform pre-strengthening treatment on the W-state 7xxx series aluminum alloy billet to obtain pre-strengthened aluminum alloy billet;
[0032] In step S1, the method for obtaining the W-state 7xxx series aluminum alloy billet is to perform a solution treatment on the aluminum alloy billet to obtain the W-state 7xxx series aluminum alloy billet. It should be understood that the solution treatment step can be performed by the aluminum alloy billet supplier and does not need to be performed by the component manufacturer.
[0033] In step S1, the W-state 7xxx series aluminum alloy billet undergoes pre-strengthening treatment to obtain a pre-strengthened aluminum alloy billet. The pre-strengthening treatment temperature is 50-150℃, and the pre-strengthening treatment time is 1-24 hours. This pre-strengthening treatment step can also be performed by the aluminum alloy billet supplier, eliminating the need for component manufacturers. The pre-strengthened aluminum alloy billet is in a stable microstructure, facilitating transportation, storage, and other operations, and exhibiting good adaptability to practical engineering applications.
[0034] S2. The pre-strengthened aluminum alloy billet is heated and held at a certain temperature, wherein the holding time is determined according to the heating temperature and the loading rate of the forming mold used subsequently.
[0035] Please refer to Figure 2 In step S2, the heating temperature and holding time are determined based on the loading rate of the forming mold used subsequently, specifically:
[0036] (1) If the loading rate of the forming die is 0.1-10s -1 When the heating temperature of the pre-strengthened aluminum alloy billet is 150-200℃, the holding time is 5-30 minutes; when the heating temperature of the pre-strengthened aluminum alloy billet is 200-250℃, the holding time is 1-20 minutes.
[0037] (2) If the loading rate of the forming die is 0.001-0.1s -1 When the heating temperature of the pre-strengthened aluminum alloy billet is 150-200℃, the holding time is 3-20 minutes; when the heating temperature of the pre-strengthened aluminum alloy billet is 200-250℃, the holding time is 0-15 minutes.
[0038] (3) If the loading rate of the forming die is less than 0.001s -1 When the heating temperature of the pre-strengthened aluminum alloy billet is 150-200℃, the holding time is 1-15 minutes; when the heating temperature of the pre-strengthened aluminum alloy billet is 200-250℃, the holding time is 0-10 minutes.
[0039] The reason why the holding time needs to be determined based on the heating temperature and the loading rate of the forming mold used later is that, firstly, different strain rates (i.e., loading rates) will cause different mechanical responses in the material. Matching the temperature and holding time in the forming process is necessary to ensure that the precipitates in the aluminum alloy are fully precipitated without coarsening or transformation, thus obtaining excellent mechanical properties. Secondly, different strain rates result in different plastic work during the deformation process, which leads to different precipitation behavior of the precipitates, dislocation movement, and interactions between the precipitates and dislocations in the aluminum alloy. Therefore, when heating and holding pre-strengthened aluminum alloy billets, it is necessary to ensure that the heating temperature and holding time are matched with the loading rate of the forming mold used later, so that the precipitates in the aluminum alloy are fully precipitated without coarsening or transformation, thereby achieving the best performance of the final aluminum alloy component.
[0040] Meanwhile, the heating temperature or holding time is also affected by the thickness of the aluminum alloy billet. If an air furnace is used for heating, the greater the thickness of the pre-strengthened aluminum alloy billet, the longer the heating time is required.
[0041] It should be noted that when the holding time is 0, it means that the heating and holding in step S2 is not performed, and the pre-strengthened aluminum alloy billet is directly cold-formed. When cold forming, the coordinated control of strain rate should be considered, and variable strain rate loading can also be used.
[0042] If the final component after molding still needs to undergo a baking paint treatment, the heat preservation time in step S2 should be shortened. This is because the component will also be subjected to heat during the baking paint treatment. Therefore, in order to avoid excessive heat to the component leading to a decrease in strength, the heat preservation time needs to be shortened.
[0043] S3. The heated and heat-insulated aluminum alloy billet is shaped using a forming mold to obtain the final component. The temperature of the forming mold is determined by the loading rate of the forming mold.
[0044] Specifically:
[0045] If the loading rate of the forming die is between 0.005 and 10 s -1 In this case, the forming mold can be a cold mold or a warm mold;
[0046] If the loading rate of the forming die is less than 0.005s -1 If so, a warm mold is used for forming.
[0047] This is because if the billet is heated and kept at a constant temperature before being transferred, there will be a temperature drop during the transfer and forming process. If the loading rate of the forming mold is large, the temperature drop will be small, and either a cold mold or a warm mold can be used. If the loading rate of the forming mold is small, the forming process will need to last longer, and the temperature drop will be more significant. In this case, a warm mold is needed to maintain the temperature of the billet.
[0048] The temperature of the warm mold is not higher than the heating temperature in step S2. Specifically, the temperature of the warm mold is 0-50°C lower than the heating temperature in step S2.
[0049] In step S3, the loading rate of the forming mold is constant or variable.
[0050] It should be noted that if the forming mold in step S3 has a self-heating function (such as an electric heating mold), the heating and heat preservation process in step S2 can be carried out directly in the forming mold; if the forming mold in step S3 does not have a self-heating function, the aluminum alloy billet needs to be heated and heat-preserved first, and then quickly transferred to the forming mold. Both of these methods fall within the protection scope of this invention.
[0051] The present invention will now be described in detail with reference to specific embodiments.
[0052] Example 1:
[0053] A method for pre-strengthening high-temperature forming of 7xxx series aluminum alloys based on loading rate includes the following steps:
[0054] (1) The W-state 7075 aluminum alloy sheet blank is pre-strengthened at a temperature of 50-100℃ for 12 hours.
[0055] (2) The aluminum alloy sheet is stamped and formed with a strain rate of approximately 0.1-10 s. -1 Heat the pre-strengthened sheet to 150-200℃ and hold for 5 minutes;
[0056] (3) Transfer the blank to a water-cooled mold for forming;
[0057] (4) Obtain the final component.
[0058] Tensile specimens were cut from the final component and subjected to uniaxial tensile tests to test its mechanical properties after forming. The average value of multiple tensile specimens was taken. The tensile strength was about 561 MPa and the yield strength was about 487 MPa (as shown in Table 1).
[0059] Example 2:
[0060] A method for pre-strengthening high-temperature forming of 7xxx series aluminum alloys based on loading rate includes the following steps:
[0061] (1) The W-state 7075 aluminum alloy sheet blank is pre-strengthened at a temperature of 50-100℃ for 12 hours.
[0062] (2) The aluminum alloy sheet is stamped and formed with a strain rate of approximately 0.1-10 s. -1 Heat the pre-strengthened sheet to 150-200℃ and hold for 15 minutes;
[0063] (3) Transfer the blank to a water-cooled mold for forming;
[0064] (4) Obtain the final component.
[0065] Tensile specimens were cut from the final component and subjected to uniaxial tensile tests to test its mechanical properties after forming. The average value of multiple tensile specimens was taken. The tensile strength was about 571 MPa and the yield strength was about 502 MPa (as shown in Table 1).
[0066] Example 3:
[0067] A method for pre-strengthening high-temperature forming of 7xxx series aluminum alloys based on loading rate includes the following steps:
[0068] (1) The W-state 7075 aluminum alloy sheet blank is pre-strengthened at a temperature of 50-100℃ for 12 hours.
[0069] (2) The aluminum alloy sheet is stamped and formed with a strain rate of approximately 0.1-10 s. -1Heat the pre-strengthened sheet to 200-250℃ and hold for 3 minutes;
[0070] (3) Transfer the blank to a water-cooled mold for forming;
[0071] (4) Obtain the final component.
[0072] Tensile specimens were cut from the final component and subjected to uniaxial tensile tests to test its mechanical properties after forming. The average value of multiple tensile specimens was taken. The tensile strength was about 566 MPa and the yield strength was about 499 MPa (as shown in Table 1).
[0073] Example 4:
[0074] A method for pre-strengthening high-temperature forming of 7xxx series aluminum alloys based on loading rate includes the following steps:
[0075] (1) The W-state 7075 aluminum alloy sheet blank is pre-strengthened at a temperature of 50-100℃ for 12 hours.
[0076] (2) The aluminum alloy sheet is stamped and formed with a strain rate of approximately 0.1-10 s. -1 Heat the pre-strengthened sheet to 200-250℃ and hold for 8 minutes;
[0077] (3) Transfer the blank to a water-cooled mold for forming;
[0078] (4) Obtain the final component.
[0079] Tensile specimens were cut from the final component and subjected to uniaxial tensile tests to test its mechanical properties after forming. The average value of multiple tensile specimens was taken. The tensile strength was about 575 MPa and the yield strength was about 507 MPa (as shown in Table 1).
[0080] Example 5:
[0081] A method for pre-strengthening high-temperature forming of 7xxx series aluminum alloys based on loading rate includes the following steps:
[0082] (1) The W-state 7A09 aluminum alloy profile blank is pre-strengthened at a temperature of 70-120℃ for 8 hours.
[0083] (2) The aluminum alloy profile is stretched and bent at a strain rate of approximately 0.001-0.01 s. -1 Heat the pre-strengthened profile to 150-200℃ and hold for 5 minutes;
[0084] (3) Transfer the blank to a warm mold for forming. The mold temperature is 100-200℃.
[0085] (4) Obtain the final component.
[0086] Tensile specimens were cut from the final component and subjected to uniaxial tensile tests to test its mechanical properties after forming. The average value of multiple tensile specimens was taken. The tensile strength was about 581 MPa and the yield strength was about 497 MPa (as shown in Table 1).
[0087] Example 6:
[0088] A method for pre-strengthening high-temperature forming of 7xxx series aluminum alloys based on loading rate includes the following steps:
[0089] (1) The W-state 7A09 aluminum alloy profile blank is pre-strengthened at a temperature of 70-120℃ for 8 hours.
[0090] (2) The aluminum alloy profile is stretched and bent at a strain rate of approximately 0.001-0.01 s. -1 Heat the pre-strengthened profile to 150-200℃ and hold for 10 minutes;
[0091] (3) Transfer the blank to a warm mold for forming. The mold temperature is 100-200℃.
[0092] (4) Obtain the final component.
[0093] Tensile specimens were cut from the final component and subjected to uniaxial tensile tests to test its mechanical properties after forming. The average value of multiple tensile specimens was taken. The tensile strength was about 597 MPa and the yield strength was about 512 MPa (as shown in Table 1).
[0094] Example 7:
[0095] A method for pre-strengthening high-temperature forming of 7xxx series aluminum alloys based on loading rate includes the following steps:
[0096] (1) The W-state 7A09 aluminum alloy profile blank is pre-strengthened at a temperature of 70-120℃ for 8 hours.
[0097] (2) The aluminum alloy profile is stretched and bent at a strain rate of approximately 0.001-0.01 s. -1 Heat the pre-strengthened profile to 200-250℃ and hold for 3 minutes;
[0098] (3) Transfer the blank to a warm mold for forming. The mold temperature is 150-250℃.
[0099] (4) Obtain the final component.
[0100] Tensile specimens were cut from the final component and subjected to uniaxial tensile tests to test its mechanical properties after forming. The average value of multiple tensile specimens was taken. The tensile strength was about 583 MPa and the yield strength was about 505 MPa (as shown in Table 1).
[0101] Example 8:
[0102] A method for pre-strengthening high-temperature forming of 7xxx series aluminum alloys based on loading rate includes the following steps:
[0103] (1) The W-state 7A09 aluminum alloy profile blank is pre-strengthened at a temperature of 70-120℃ for 8 hours.
[0104] (2) The aluminum alloy profile is stretched and bent at a strain rate of approximately 0.001-0.01 s. -1 Heat the pre-strengthened profile to 200-250℃ and hold for 6 minutes;
[0105] (3) Transfer the blank to a warm mold for forming. The mold temperature is 150-250℃.
[0106] (4) Obtain the final component.
[0107] Tensile specimens were cut from the final component and subjected to uniaxial tensile tests to test its mechanical properties after forming. The average value of multiple tensile specimens was taken. The tensile strength was about 606 MPa and the yield strength was about 525 MPa (as shown in Table 1).
[0108] Comparative Example 1:
[0109] A method for pre-strengthening high-temperature forming of 7xxx series aluminum alloys based on loading rate includes the following steps:
[0110] (1) The W-state 7075 aluminum alloy sheet blank is pre-strengthened at a temperature of 50-100℃ for 12 hours.
[0111] (2) The aluminum alloy sheet is stamped and formed with a strain rate of approximately 0.1-10 s. -1 Heat the pre-strengthened sheet to 150-200℃ and hold for 2 minutes;
[0112] (3) Transfer the blank to a water-cooled mold for forming;
[0113] (4) Obtain the final component.
[0114] Tensile specimens were cut from the final component and subjected to uniaxial tensile tests to test its mechanical properties after forming. The average value of multiple tensile specimens was taken. The tensile strength was about 514 MPa and the yield strength was about 442 MPa (as shown in Table 1).
[0115] Comparative Example 2:
[0116] A method for pre-strengthening high-temperature forming of 7xxx series aluminum alloys based on loading rate includes the following steps:
[0117] (1) The W-state 7075 aluminum alloy sheet blank is pre-strengthened at a temperature of 50-100℃ for 12 hours.
[0118] (2) The aluminum alloy sheet is stamped and formed with a strain rate of approximately 0.1-1s. -1 Heat the pre-strengthened sheet to 200-250℃ and hold for 30 minutes;
[0119] (3) Transfer the blank to a water-cooled mold for forming;
[0120] (4) Obtain the final component.
[0121] Tensile specimens were cut from the final component and subjected to uniaxial tensile tests to test its mechanical properties after forming. The average value of multiple tensile specimens was taken. The tensile strength was about 543 MPa and the yield strength was about 461 MPa (as shown in Table 1).
[0122] Comparative Example 3:
[0123] A method for pre-strengthening high-temperature forming of 7xxx series aluminum alloys based on loading rate includes the following steps:
[0124] (1) The W-state 7A09 aluminum alloy profile blank is pre-strengthened at a temperature of 70-120℃ for 8 hours.
[0125] (2) The aluminum alloy profile is stretched and bent at a strain rate of approximately 0.001-0.01 s. -1 Heat the pre-strengthened profile to 150-200℃ and hold for 50 seconds;
[0126] (3) Transfer the blank to a warm mold for forming. The mold temperature is 100-200℃.
[0127] (4) Obtain the final component.
[0128] Tensile specimens were cut from the final component and subjected to uniaxial tensile tests to test its mechanical properties after forming. The average value of multiple tensile specimens was taken. The tensile strength was about 529 MPa and the yield strength was about 454 MPa (as shown in Table 1).
[0129] Comparative Example 4:
[0130] A method for pre-strengthening high-temperature forming of 7xxx series aluminum alloys based on loading rate includes the following steps:
[0131] (1) The W-state 7A09 aluminum alloy profile blank is pre-strengthened at a temperature of 70-120℃ for 8 hours.
[0132] (2) The aluminum alloy profile is stretched and bent at a strain rate of approximately 0.001-0.01 s. -1 Heat the pre-strengthened profile to 200-250℃ and hold for 30 minutes;
[0133] (3) Transfer the blank to a warm mold for forming. The mold temperature is 150-250℃.
[0134] (4) Obtain the final component.
[0135] Tensile specimens were cut from the final component and subjected to uniaxial tensile tests to test its mechanical properties after forming. The average value of multiple tensile specimens was taken, and its tensile strength was about 509 MPa and its yield strength was about 432 MPa.
[0136] Table 1 Summary of mechanical properties of parts in the examples and comparative examples.
[0137]
[0138] In the embodiments and comparative examples of the present invention, the mechanical properties of the parts obtained after warm forming under different strain rates and process parameters are summarized in Table 1. As can be seen from Table 1, when aluminum alloy pre-strengthening forming is carried out using the technical solution provided by the present invention, it has better mechanical properties than the comparative example.
[0139] The beneficial effects of the technical solution provided by this invention include:
[0140] (1) The forming process disclosed in this invention fully considers the loading rate of different parts and different forming methods as well as the equipment conditions of forming molds. The process parameters of heating and heat preservation and molding are customized to match the heating temperature and heat preservation time with the subsequent forming loading rate, so that the precipitated phase in the aluminum alloy is fully precipitated and does not coarsen or transform, thereby making the final aluminum alloy component achieve the best performance.
[0141] (2) This invention fully considers the entire process strategy for the production of different parts, closely integrating the forming process parameters with subsequent processes such as painting, and has high production applicability. At the same time, since subsequent painting and other processes include heat treatment, the coordination between processes can achieve high strength of the parts in the final service state;
[0142] (3) The pre-strengthening process can be completed by the aluminum alloy billet supplier without the need for the parts manufacturer, which simplifies the production process; and the pre-strengthened aluminum alloy billet is in a stable state, which is convenient for transportation, storage and other operations, and has good adaptability to actual engineering.
[0143] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for pre-strengthening and forming 7xxx series aluminum alloys based on loading rate, characterized in that, Includes the following steps: S1. Obtain W-state 7xxx series aluminum alloy billet, and perform pre-strengthening treatment on the W-state 7xxx series aluminum alloy billet to obtain pre-strengthened aluminum alloy billet; S2. The pre-strengthened aluminum alloy billet is heated and held at a certain temperature, wherein the holding time is determined according to the heating temperature and the loading rate of the forming mold used subsequently. S3. The heated and heat-insulated aluminum alloy billet is shaped using a forming mold to obtain the final component. The temperature of the forming mold is determined by the loading rate of the forming mold. In step S1, the pre-strengthened aluminum alloy billet of W state 7xxx series is pre-strengthened to obtain pre-strengthened aluminum alloy billet. The pre-strengthened treatment temperature is 50-150℃ and the pre-strengthened treatment time is 1-24h. In step S2, the holding time is determined based on the heating temperature and the loading rate of the forming mold used subsequently, specifically as follows: (1) If the loading rate of the forming die is 0.1-10s -1 When the heating temperature of the pre-strengthened aluminum alloy billet is 150-200℃, the holding time is 5-30 minutes; when the heating temperature of the pre-strengthened aluminum alloy billet is 200-250℃, the holding time is 1-20 minutes. (2) If the loading rate of the forming die is 0.001-0.1s -1 When the heating temperature of the pre-strengthened aluminum alloy billet is 150-200℃, the holding time is 3-20 minutes; when the heating temperature of the pre-strengthened aluminum alloy billet is 200-250℃, the holding time is 0-15 minutes. (3) If the loading rate of the forming die is less than 0.001s -1 When the heating temperature of the pre-strengthened aluminum alloy billet is 150-200℃, the holding time is 1-15 minutes; when the heating temperature of the pre-strengthened aluminum alloy billet is 200-250℃, the holding time is 0-10 minutes. In step S3, the temperature of the forming mold is determined by the loading rate of the forming mold, specifically: If the loading rate of the forming die is between 0.005 and 10 s -1 In this case, the forming mold can be a cold mold or a warm mold; If the loading rate of the forming die is less than 0.005s -1 If so, a warm mold is used for forming.
2. The method for pre-strengthening 7xxx series aluminum alloys based on loading rate according to claim 1, characterized in that, In step S2, if an air furnace is used for heating, the greater the thickness of the pre-strengthened aluminum alloy billet, the longer the heating time is required.
3. The method for pre-strengthening 7xxx series aluminum alloys based on loading rate according to claim 1, characterized in that, If the final component after forming still needs to undergo a baking paint process, the heat preservation time in step S2 should be shortened.
4. The method for pre-strengthening 7xxx series aluminum alloys based on loading rate according to claim 1, characterized in that, The temperature of the mold should not be higher than the heating temperature in step S2.
5. The method for pre-strengthening 7xxx series aluminum alloys based on loading rate according to claim 4, characterized in that, The temperature of the mold is 0-50°C lower than the heating temperature in step S2.
6. The method for pre-strengthening 7xxx series aluminum alloys based on loading rate according to claim 1, characterized in that, In step S1, the method for obtaining the W-state 7xxx series aluminum alloy billet is to perform a solution treatment on the aluminum alloy billet to obtain the W-state 7xxx series aluminum alloy billet.
7. The method for pre-strengthening 7xxx series aluminum alloys based on loading rate according to claim 1, characterized in that, In step S3, the loading rate of the forming mold is constant or variable.
Citation Information
Patent Citations
Aluminum alloy pre-strengthening hot stamping forming method
CN112264498A
Method for reducing thermoplastic deformation resistance of spray-formed aluminum alloy
CN114457297A