PVDF binder and its use in the preparation of cathodes for batteries

Through the synergistic effect of the first PVDF copolymer and the second PVDF homopolymer, the chain reaction of PVDF under strong alkali is suppressed, which solves the problem of insufficient alkali resistance of PVDF binder in high-alkalinity ternary cathode or sodium battery cathode systems, realizes the stability and electronic conductivity of battery cathode slurry, and improves electrode adhesion.

CN117603634BActive Publication Date: 2026-11-24RUYUAN DONGYANG LIGHT FLUORINE RESIN CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311372400.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-20
Publication Date
2026-11-24
Estimated Expiration
2043-10-20

AI Technical Summary

Technical Problem

Existing PVDF binders have insufficient alkali resistance in highly alkaline ternary cathode or sodium battery cathode systems, and are prone to gelation, affecting the stability and lifespan of the battery.

Method used

The combination of a first PVDF copolymer and a second PVDF homopolymer is used. By copolymerizing fluorinated monomers with VDF, the chain reaction of PVDF under strong alkali is suppressed. Combined with the high branching degree of the second PVDF homopolymer, the stability and electronic conductivity of the slurry are guaranteed.

Benefits of technology

It significantly improves the alkali resistance of PVDF binder in high-alkaline systems, maintains the uniformity and stability of active material slurry, enhances the adhesion of positive electrode sheets, and extends the battery's lifespan and capacity maintenance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117603634B_ABST
    Figure CN117603634B_ABST
Patent Text Reader

Abstract

This invention discloses a PVDF binder and its application in the preparation of battery cathodes, relating to the field of new energy battery technology. The PVDF binder of this invention comprises a first PVDF copolymer and a second PVDF homopolymer. The first PVDF copolymer is copolymerized from VDF monomers and fluorinated monomers, wherein the content of the fluorinated monomers is 5-20% of the VDF monomer content. The branching degree of the second PVDF homopolymer is 5-25 / 1000C, and the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 0.5:9.5-4:6. Through the synergistic effect of the first PVDF copolymer and the second PVDF homopolymer, this invention can significantly improve the alkali resistance of the PVDF binder in highly alkaline ternary cathode or sodium battery cathode systems, maintain the uniformity and stability of the active material during slurry preparation, and greatly enhance the adhesion of the cathode sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of new energy battery technology, and more specifically, to a PVDF binder and its application in the preparation of battery cathodes. Background Technology

[0002] PVDF binders can bond active materials (lithium iron phosphate, ternary cathode materials, sodium-ion cathode materials, etc.), conductive agents, and current collectors on the positive electrode of a battery. They maintain the uniformity and stability of the active material slurry during preparation and provide the necessary electron conduction within the electrode, playing a crucial role in maintaining battery capacity, lifespan, and stability. Homopolymerized PVDF has poor adhesion and poor alkali resistance in ternary cathode slurries and sodium-ion cathodes, easily leading to gelation. To improve the adhesion of PVDF and its alkali resistance in high-alkaline power battery systems, polar comonomers, such as acrylic acid and maleic anhydride ester monomers, are typically introduced into PVDF. Currently, the polar comonomers used in copolymerized PVDF contain carboxyl groups, which, while providing good adhesion in ternary power battery systems (NCM523, NCM811), still exhibit gelation and poor alkali resistance in even more alkaline ternary cathodes (nickel content exceeding 90%) or sodium-ion battery cathode systems, even with further increases in the carboxyl group copolymer content.

[0003] Existing technology discloses a vinylidene fluoride copolymer containing vinylidene fluoride monomer and at least one modified maleic ester monomer. The modified maleic ester monomer accounts for more than 0-20% of the total monomer mass. The copolymer of monomethyl maleate and vinylidene fluoride has significantly improved adhesion compared to the homopolymer of vinylidene fluoride. However, due to its shorter side chain length, there is still considerable room for improvement in adhesion performance. When the number of side chain atoms is 4-10, it has better side chain flexibility. At the same time, more O, S, N, Cl, and Br atoms can provide more bonding sites. The combined effect of these two factors can significantly improve the adhesion performance of the polymer. Although the existing technology discloses copolymer modification of PVDF with the introduction of maleic anhydride ester monomers improves the adhesion performance, it does not solve the problem of insufficient alkali resistance and easy gelation of PVDF binder in highly alkaline ternary cathode or sodium battery cathode systems.

[0004] Therefore, there is an urgent need in this field to develop a PVDF binder that can be applied to high-alkalinity ternary cathode or sodium battery cathode systems. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to overcome the defect of insufficient alkali resistance of existing PVDF binders in highly alkaline ternary cathode or sodium battery cathode systems, and to provide a PVDF binder comprising a first PVDF copolymer and a second PVDF homopolymer, which can significantly inhibit the chain reaction of PVDF de-HF under strong alkali (high nickel ternary cathode, sodium battery cathode), ensure the stability of the cathode slurry and prevent gelation.

[0006] Another object of the present invention is to provide an application of PVDF binder in the preparation of battery cathode.

[0007] Another object of the present invention is to provide an electrode composition.

[0008] The above-mentioned objective of this invention is achieved through the following technical solution:

[0009] A PVDF adhesive comprising a first PVDF copolymer and a second PVDF homopolymer,

[0010] The first PVDF copolymer is formed by copolymerizing VDF monomers and fluorinated monomers. The main structure of the fluorinated monomers is as follows:

[0011]

[0012] Wherein R is a C1-C4 fluorinated alkyl group or an alkyl group substituted with at least one heteroatom selected from O, N, P, S, Cl, Br, and I, and the content of the fluorinated monomer is 5-20% of the VDF monomer content.

[0013] The degree of branching of the second PVDF homopolymer is 5–25 / 1000°C.

[0014] The mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:1.5 to 1:18.

[0015] It should be noted that:

[0016] PVDF gelation mechanism, such as Figure 1 :

[0017] PVDF undergoes a chain reaction of HF removal under the influence of strong bases, resulting in the formation of chained double bonds in the main chain. The gelation phenomenon may be caused by the splitting of double bonds, the generation of carbon free radicals on the polymer main chain, and their recombination with other molecules.

[0018] This invention, by selecting fluorine-containing monomers to copolymerize with VDF, can significantly suppress the chain reaction of HF removal from PVDF under strong alkaline conditions (high-nickel ternary cathode, sodium battery cathode), ensuring the stability of the cathode slurry and preventing gelation.

[0019] The second PVDF homopolymer has a high degree of branching, which can play a good dispersing role and ensure that the slurry will not settle.

[0020] Through the synergistic effect of the first PVDF copolymer and the second PVDF homopolymer, the alkali resistance of PVDF binder in highly alkaline ternary cathode or sodium battery cathode systems can be significantly improved, the uniformity and stability of active material slurry can be maintained, and the electron conduction required in the electrode can be provided, which plays a vital role in maintaining battery capacity, service life and stability.

[0021] The R of the fluorinated monomer in the first PVDF copolymer is an alkyl group substituted with at least one heteroatom from O, N, P, S, Cl, Br, I, which can provide more bonding sites.

[0022] In the first PVDF copolymer, the content of the fluorinated monomer is 5-20% of the VDF monomer content. If the content of the fluorinated monomer is too high, the overall crystallinity decreases, and the PVDF becomes less resistant to electrolytes; if the content of the fluorinated monomer is too low, it does not have the effect of alkali resistance.

[0023] The present invention also requires controlling the mass ratio of the first PVDF copolymer and the second PVDF homopolymer to be 1:1.5 to 1:18. If there is too much first PVDF copolymer, the overall adhesive strength will be reduced, and if there is too little first PVDF copolymer, the alkali resistance will be poor.

[0024] In this invention, the copolymerization of VDF with fluorinated monomers can be carried out by emulsion polymerization or suspension polymerization, with suspension polymerization being preferred.

[0025] The preparation method of PVDF copolymer can be referred to as follows:

[0026] In the reaction system, a dispersant and deionized water are added, and the system is evacuated until the oxygen content is less than 10 ppm.

[0027] Heat and stir, add some VDF monomer, and maintain a reaction pressure;

[0028] The polymerization reaction begins with the addition of an initiator and a chain transfer agent, and the comonomer is continuously added to the reactor.

[0029] After the reaction is complete, the product is washed and dried to obtain polyvinylidene fluoride copolymer resin powder.

[0030] The polymerization initiator of this invention can be an organic peroxide initiator, such as diisopropyl peroxide dicarbonate, di-n-propyl peroxide dicarbonate, diisobutyryl peroxide, tert-butyl peroxypentanoate, or tert-amyl peroxypentanoate. The emulsion polymerization system can also use a persulfate or persulfate / sodium bisulfite initiation system, preferably an ammonium persulfate initiation system.

[0031] Chain transfer agents can be added to the polymerization system of the present invention to adjust the molecular weight of the polymer. Chemicals that can be used for chain transfer include ethyl acetate, diethyl malonate, diethyl carbonate, dimethyl carbonate, acetone, ethanol, n-propanol, etc. The chain transfer agent accounts for 0.01%-1% of the mass fraction of the polymer monomer.

[0032] In a specific embodiment, the content of the fluorinated monomer is preferably 10-15% of the VDF monomer content.

[0033] In a specific embodiment, preferably, the weight-average molecular weight of the first PVDF copolymer is between 2 million and 5 million.

[0034] The first PVDF copolymer has a very high molecular weight, which can greatly improve the adhesion of the positive electrode sheet.

[0035] Preferably, the degree of branching of the second PVDF homopolymer is 10 to 20 / 1000C.

[0036] In a specific embodiment, preferably, the weight-average molecular weight of the second PVDF homopolymer is 600,000 to 1,000,000. The weight-average molecular weight of the second PVDF homopolymer can further improve the adhesion between the PVDF binder and the electrode.

[0037] Preferably, the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:4 to 1:9.

[0038] The present invention also specifically protects the application of the PVDF binder in the preparation of battery cathodes.

[0039] The PVDF binder of this invention not only has good bonding performance, but also can significantly inhibit the chain reaction of PVDF de-HF under strong alkali, ensuring the stability of the cathode slurry, preventing gelation, maintaining the uniformity and stability of the active material during slurry preparation, and providing the electron conduction required within the electrode. It can meet the application requirements of various battery cathode systems and can be widely used in battery cathode preparation.

[0040] In specific applications, it exhibits good stability, especially in sodium battery cathode systems and high-alkaline battery cathodes with a nickel content of ≥90%.

[0041] The present invention also specifically protects an electrode composition comprising an electrode material, a conductive agent, and the PVDF binder.

[0042] In a specific embodiment, preferably, the mass fractions of each component in the electrode composition are: 96-99 parts of electrode material, 0.3-1 part of conductive agent, and 0.5-3 parts of PVDF binder.

[0043] Compared with the prior art, the beneficial effects of the present invention are:

[0044] The present invention, through the synergistic effect of the first PVDF copolymer and the second PVDF homopolymer, can significantly improve the alkali resistance of PVDF binder in highly alkaline ternary cathode or sodium battery cathode systems, maintain the uniformity and stability of active material slurry preparation, and greatly enhance the adhesion of cathode sheet. Attached Figure Description

[0045] Figure 1 This is a diagram illustrating the gelation mechanism of PVDF. Detailed Implementation

[0046] The present invention will be further described below with reference to specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise stated, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.

[0047] Example 1

[0048] A PVDF adhesive comprises a first PVDF copolymer and a second PVDF homopolymer, wherein the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:4.

[0049] The weight-average molecular weight of the first PVDF copolymer is 3 million;

[0050] The weight-average molecular weight of the second PVDF homopolymer is 700,000.

[0051] The first PVDF copolymer is copolymerized from VDF monomer and fluorinated monomer, wherein the fluorinated monomer is hexafluoropropylene and the content of the fluorinated monomer is 10% of the VDF monomer content. The preparation method is as follows:

[0052] First method for preparing PVDF copolymer:

[0053] In a 20L vertical polymerization reactor, 10kg of deionized water and 4g of methylcellulose were added. The reactor was closed, evacuated, and purged several times with nitrogen until the oxygen content inside the reactor was less than 10ppm. 4.5kg of a VDF / fluorinated monomer mixture was added to bring the reactor pressure to 6.0MPa. The reactor was heated to 45℃, and the stirrer was started at 800r / min. After reacting for 6 hours, the reactor was depressurized, the suspension was collected, and repeatedly washed until the conductivity of the filtrate dropped below 0.1. Finally, the mixture was dried in a 95℃ oven for 24 hours to obtain polyvinylidene fluoride copolymer resin powder.

[0054] The second PVDF homopolymer has a branching degree of 10 / 1000C, and its preparation method is as follows:

[0055] In a 20L vertical polymerization reactor, 11.5 kg of deionized water was added. The reactor was closed, evacuated, and purged several times with nitrogen until the oxygen content inside the reactor was less than 10 ppm. The reactor was heated to 100°C, and the stirrer was turned on at a speed of 400 r / min. A certain amount of VDF monomer was added to bring the reactor pressure to 4.1 MPa. 6.4 g of ammonium persulfate and 34.8 g of diethyl malonate were added to the reactor using an additive pump at a rate of 150 g / h. Simultaneously, the polymerization reaction began, and the reaction pressure was maintained constant by continuously adding VDF monomer. After 1 hour of reaction, 2.8 g of ammonium persulfate was added, and after 2 hours of reaction, another 2.8 g of ammonium persulfate and 9.3 g of diethyl malonate were added. When the amount of VDF monomer reacted reached 3 kg, the reaction was stopped, and the reaction time was 4.7 hours. The reactor was depressurized, the emulsion was collected, broken, and repeatedly washed until the conductivity of the filtrate dropped below 0.1. Finally, the product was dried in an oven at 95°C for 24 hours to obtain polyvinylidene fluoride copolymer resin powder.

[0056] Example 2

[0057] A PVDF adhesive comprises a first PVDF copolymer and a second PVDF homopolymer, wherein the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:4.

[0058] The weight-average molecular weight of the first PVDF copolymer is 3 million;

[0059] The weight-average molecular weight of the second PVDF homopolymer is 700,000.

[0060] The first PVDF copolymer is copolymerized from VDF monomer and fluorinated monomer, wherein the fluorinated monomer is hexafluoropropylene and the content of the fluorinated monomer is 20% of the VDF monomer content. The preparation method is as follows:

[0061] The preparation method of the first PVDF copolymer is the same as in Example 1.

[0062] The second PVDF homopolymer has a branching degree of 10 / 1000C and is prepared using the same method as in Example 1.

[0063] Example 3

[0064] A PVDF adhesive comprises a first PVDF copolymer and a second PVDF homopolymer, wherein the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:9.

[0065] The weight-average molecular weight of the first PVDF copolymer is 3 million;

[0066] The weight-average molecular weight of the second PVDF homopolymer is 700,000.

[0067] The first PVDF copolymer is copolymerized from VDF monomer and fluorinated monomer, wherein the fluorinated monomer is hexafluoropropylene and the content of the fluorinated monomer is 20% of the VDF monomer content. The preparation method is as follows:

[0068] The preparation method of the first PVDF copolymer is the same as in Example 1.

[0069] The second PVDF homopolymer has a branching degree of 10 / 1000C and is prepared using the same method as in Example 1.

[0070] Example 4

[0071] A PVDF adhesive comprises a first PVDF copolymer and a second PVDF homopolymer, wherein the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:4.

[0072] The weight-average molecular weight of the first PVDF copolymer is 3 million;

[0073] The weight-average molecular weight of the second PVDF homopolymer is 700,000.

[0074] The first PVDF copolymer is copolymerized from VDF monomer and fluorinated monomer. The fluorinated monomer is trifluorochloroethylene, and the content of the fluorinated monomer is 20% of the content of VDF monomer. The preparation method is the same as in Example 1.

[0075] Example 5

[0076] A PVDF adhesive comprises a first PVDF copolymer and a second PVDF homopolymer, wherein the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:1.5.

[0077] The weight-average molecular weight of the first PVDF copolymer is 3 million;

[0078] The weight-average molecular weight of the second PVDF homopolymer is 700,000.

[0079] The first PVDF copolymer is copolymerized from VDF monomer and fluorinated monomer, with the fluorinated monomer being hexafluoropropylene and the content of the fluorinated monomer being 20% ​​of the VDF monomer content.

[0080] The preparation method of the first PVDF copolymer is the same as in Example 1.

[0081] The second PVDF homopolymer has a branching degree of 10 / 1000C and is prepared using the same method as in Example 1.

[0082] Example 6

[0083] A PVDF adhesive comprises a first PVDF copolymer and a second PVDF homopolymer, wherein the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:18.

[0084] The weight-average molecular weight of the first PVDF copolymer is 3 million;

[0085] The weight-average molecular weight of the second PVDF homopolymer is 700,000.

[0086] The first PVDF copolymer is copolymerized from VDF monomer and fluorinated monomer, with the fluorinated monomer being hexafluoropropylene and the content of the fluorinated monomer being 20% ​​of the VDF monomer content.

[0087] The preparation method of the first PVDF copolymer is the same as in Example 1.

[0088] The second PVDF homopolymer has a branching degree of 10 / 1000C and is prepared using the same method as in Example 1.

[0089] Example 7

[0090] A PVDF adhesive comprises a first PVDF copolymer and a second PVDF homopolymer, wherein the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:4.

[0091] The weight-average molecular weight of the first PVDF copolymer is 3 million;

[0092] The weight-average molecular weight of the second PVDF homopolymer is 700,000.

[0093] The first PVDF copolymer is copolymerized from VDF monomer and fluorinated monomer, with the fluorinated monomer being hexafluoropropylene and the content of the fluorinated monomer being 5% of the VDF monomer content.

[0094] The preparation method of the first PVDF copolymer is the same as in Example 1.

[0095] The second PVDF homopolymer has a branching degree of 10 / 1000C and is prepared using the same method as in Example 1.

[0096] Example 8

[0097] A PVDF adhesive comprises a first PVDF copolymer and a second PVDF homopolymer, wherein the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:4.

[0098] The weight-average molecular weight of the first PVDF copolymer is 3 million;

[0099] The weight-average molecular weight of the second PVDF homopolymer is 700,000.

[0100] The first PVDF copolymer is copolymerized from VDF monomer and fluorinated monomer, wherein the fluorinated monomer is hexafluoropropylene and the content of the fluorinated monomer is 10% of the VDF monomer content. The preparation method is as follows:

[0101] The preparation method of the first PVDF copolymer is the same as in Example 1.

[0102] The second PVDF homopolymer has a branching degree of 5 / 1000C and is prepared using the same method as in Example 1.

[0103] Example 9

[0104] A PVDF adhesive comprises a first PVDF copolymer and a second PVDF homopolymer, wherein the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:4.

[0105] The weight-average molecular weight of the first PVDF copolymer is 3 million;

[0106] The weight-average molecular weight of the second PVDF homopolymer is 700,000.

[0107] The first PVDF copolymer is copolymerized from VDF monomer and fluorinated monomer, wherein the fluorinated monomer is hexafluoropropylene and the content of the fluorinated monomer is 10% of the VDF monomer content. The preparation method is as follows:

[0108] The preparation method of the first PVDF copolymer is the same as in Example 1.

[0109] The second PVDF homopolymer has a branching degree of 25 / 1000C and is prepared using the same method as in Example 1.

[0110] Comparative Example 1

[0111] A PVDF adhesive comprises a first PVDF copolymer and a second PVDF homopolymer, wherein the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:4.

[0112] The weight-average molecular weight of the first PVDF copolymer is 3 million;

[0113] The weight-average molecular weight of the second PVDF homopolymer is 700,000.

[0114] The first PVDF copolymer is copolymerized from VDF monomer and fluorinated monomer. The fluorinated monomer is hexafluoropropylene, and the content of the fluorinated monomer is 2% of the content of VDF monomer. The preparation method is the same as in Example 1.

[0115] The second PVDF homopolymer has a branching degree of 10 / 1000C and is prepared using the same method as in Example 1.

[0116] Comparative Example 2

[0117] A PVDF adhesive comprises a PVDF copolymer and a second PVDF homopolymer, wherein the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:4.

[0118] The weight-average molecular weight of the first PVDF copolymer is 3 million;

[0119] The weight-average molecular weight of the second PVDF homopolymer is 700,000.

[0120] The first PVDF copolymer is composed solely of VDF monomers and is prepared using the same method as in Example 1.

[0121] The second PVDF homopolymer has a branching degree of 10 / 1000C and is prepared using the same method as in Example 1.

[0122] Comparative Example 3

[0123] One is a PVDF homopolymer, and the preparation method of the PVDF homopolymer is the same as in Example 1.

[0124] Comparative Example 4

[0125] A PVDF adhesive includes a PVDF copolymer, which is copolymerized from VDF monomer and a fluorinated monomer. The fluorinated monomer is hexafluoropropylene, and the content of the fluorinated monomer is 2% of the content of the VDF monomer. The preparation method is the same as in Example 1.

[0126] Comparative Example 5

[0127] A PVDF adhesive comprises a first PVDF copolymer and a second PVDF homopolymer, wherein the mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:4.

[0128] The weight-average molecular weight of the first PVDF copolymer is 3 million;

[0129] The weight-average molecular weight of the second PVDF homopolymer is 700,000.

[0130] The first PVDF copolymer is copolymerized from VDF monomer and fluorinated monomer. The fluorinated monomer is hexafluoropropylene, and the content of the fluorinated monomer is 10% of the content of VDF monomer. The preparation method is the same as in Example 1.

[0131] The degree of branching of the second PVDF homopolymer is 2 / 1000C, and the preparation method is the same as in Example 1.

[0132] Result detection

[0133] The PVDF binders of the above embodiments and comparative examples were used to prepare electrode compositions, including electrode materials, conductive agents, and PVDF binders.

[0134] (1) Preparation process of positive electrode material (NCM9 system): 2g of PVDF mixture was dissolved in 100g of NMP solution and stirred until fully dissolved. Then, 2.8g of conductive carbon black and 56.2g of NCM9 / 0.5 / 0.5 were added under stirring, and ultrasonic stirring was performed for 2h to obtain a uniform slurry. The slurry was coated onto a 12μm thick aluminum foil using a coating machine. The aluminum foil was then dried in a vacuum oven at 60℃ for 12h to obtain the positive electrode.

[0135] (2) Sodium battery cathode system

[0136] Dissolve 2g of PVDF mixture in 100g of NMP solution and stir until fully dissolved. Then, while stirring, add 2.8g of conductive carbon black and 56.2g of sodium nickel iron manganese oxide (NaNi). 1 / 3 Fe 1 / 3 Mn 1 / 3 O2) was added and ultrasonically stirred for 2 hours to obtain a uniform slurry. The slurry was then coated onto a 12μm thick aluminum foil for the positive electrode using a coating machine. The aluminum foil was then dried in a vacuum oven at 60℃ for 12 hours to obtain the positive electrode.

[0137] The adhesive strength test was conducted according to the test method in the national standard GB / T2790-1995 "Test method for 180° peel strength of adhesives, flexible materials versus rigid materials".

[0138] Melting point is determined by the peak melting point of the polymer using DSC testing.

[0139] The specific test results are shown in Tables 1 and 2 below.

[0140] Table 1. High-alkalinity ternary cathode

[0141]

[0142]

[0143] Table 2. Sodium battery cathode system

[0144]

[0145]

[0146] As can be seen from the test results in Tables 1 and 2 above, the PVDF binder of the present invention exhibits excellent stability of the cathode slurry in both high-nickel ternary cathode and sodium battery cathode strong alkaline systems, without gelation, exhibiting a low 24-hour viscosity increase rate and uniform and stable slurry. Furthermore, the PVDF binder of the present invention maintains a bonding strength of 10.5–16.1 N / m for the cathode sheet, demonstrating good bonding strength.

[0147] Compared to the embodiments of the present invention, the content of fluorinated monomer in the first PVDF copolymer in Comparative Example 1 is 2% of the VDF monomer content. The content of fluorinated monomer is too low, which leads to severe gelation phenomenon and the bonding strength of the positive electrode sheet is only 3.0 to 3.6 N / m, which is low.

[0148] In Comparative Example 2, the first PVDF copolymer was copolymerized only from VDF monomers. The viscosity increased by 800-1000% in 24 hours, and severe gelation occurred. The bonding strength of the positive electrode was only 3.5-4.2 N / m, which is low.

[0149] Comparative Example 3 contained only the second PVDF homopolymer, while Comparative Example 4 contained only the first PVDF copolymer. Both of these showed deterioration in slurry stability and dispersibility, manifested as severe gelation and slurry sedimentation, and the bonding strength of the positive electrode sheet was also low.

[0150] In Comparative Example 5, the branching degree of the second PVDF homopolymer was 2 / 1000C, the slurry dispersibility was poor, slurry sedimentation occurred, and the bonding strength of the positive electrode sheet was also low.

[0151] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. Those skilled in the art can make other variations or modifications based on the above description. It is neither necessary nor possible to exhaustively describe all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.

Claims

1. An application of a PVDF binder in the preparation of a battery cathode, characterized in that, The positive electrode of the battery is a ternary cathode or a sodium-ion battery cathode, wherein the nickel content of the ternary cathode is ≥90% by mass. The PVDF binder comprises a first PVDF copolymer and a second PVDF homopolymer. The first PVDF copolymer is formed by copolymerizing VDF monomers and fluorinated monomers. The main structure of the fluorinated monomers is as follows: Wherein R is a C1-C4 fluorinated alkyl group or an alkyl group substituted with at least one heteroatom selected from O, N, P, S, Cl, Br, and I, and the content of the fluorinated monomer is 5-20% of the VDF monomer content. The degree of branching of the second PVDF homopolymer is 5~25 / 1000C. The mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:1.5 to 1:

18. The weight-average molecular weight of the first PVDF copolymer is between 2 million and 5 million.

2. The application as described in claim 1, characterized in that, The content of the fluorinated monomer is 10-15% of the VDF monomer content.

3. The application as described in claim 1, characterized in that, The degree of branching of the second PVDF homopolymer is 10~20 / 1000C.

4. The application as described in claim 1, characterized in that, The weight-average molecular weight of the second PVDF homopolymer is 600,000 to 1,000,000.

5. The application as described in claim 1, characterized in that, The mass ratio of the first PVDF copolymer to the second PVDF homopolymer is 1:4 to 1:9.

Citation Information

Patent Citations

  • Low gel content vinylidene fluoride thermoplastic resin, preparation method and applications thereof

    CN109721892A

  • Intermixing type binder, slurry and preparation method and application thereof

    CN115498188A