Rare earth oxide-containing slagging agent, preparation process and application thereof

By using rare earth oxide slag-forming agents in combination, the problems of slag formation difficulty and high iron loss in slag removal operations were solved, achieving the effects of rapid slag formation, easy slag removal, and low iron loss, thereby improving the quality of molten steel and production efficiency.

CN117604193BActive Publication Date: 2026-11-24HENAN TONGYU METALLURGY MATERIALS GRP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202311539574.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-18
Publication Date
2026-11-24
Estimated Expiration
2043-11-18

AI Technical Summary

Technical Problem

Existing technologies for slag removal operations suffer from difficulties in slag aggregation, fragile slag blocks, high iron loss, and severe iron entrapment in steel slag, which affect production efficiency and economic benefits.

Method used

A slag-forming agent containing rare earth oxides is used, with the main components being REO, SiO₂, Al₂O₃, CaO, MgO, and Al. Through the combination of rare earth mineral powder, lightly calcined perlite, AD powder, and dolomite powder, the desulfurization and dephosphorization properties of REO, the increased viscosity of Al₂O₃, and the increased interfacial tension of MgO are utilized to break the iron-coating phenomenon, thereby achieving rapid slag formation and low iron loss.

Benefits of technology

It achieves rapid slag accumulation and easy slag removal, reduces iron loss, avoids a decline in molten steel quality, and improves slag removal efficiency and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004556226250000131
    Figure BDA0004556226250000131
Patent Text Reader

Abstract

This invention provides a rare earth oxide-containing slag-forming agent, its preparation process, and its application, belonging to the field of metal smelting technology. The rare earth oxide-containing slag-forming agent has the following main chemical components by mass percentage: REO: 7-23%, SiO2: 29-45%, Al2O3: 13-23%, CaO: 3-7%, MgO: 2-5%, Al: 0.5-1.5%, loss on ignition: 4-9%, with the remainder being unavoidable impurities. This invention provides a rare earth oxide-containing slag-forming agent that achieves rapid slag formation, facilitates slag removal, has no negative impact on the sulfur and phosphorus fixation properties of steel slag, and significantly reduces iron loss.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal smelting technology, specifically relating to a slag-forming agent containing rare earth oxides, its preparation process, and its application. Background Technology

[0002] To improve the quality of molten steel, a series of slag-forming materials need to be added to achieve smelting tasks such as deoxidation, sulfur removal, phosphorus removal, and inclusion adsorption. Especially for specialty steels with requirements for ultra-low sulfur and high alloy content, the amount of slag-forming agent added is often very large. After completing the smelting tasks, the molten steel is then subjected to slag removal treatment before casting.

[0003] In actual production, the slag removal process has the following problems: the slag scraper has difficulty collecting slag, and the collected slag blocks are easily broken, resulting in long slag removal time and affecting the production rhythm; the phenomenon of "iron encasing" in slag is common, in which the molten iron encased in the slag will be lost during the slag removal process, resulting in significant iron loss and affecting economic benefits. Summary of the Invention

[0004] In view of this, the technical problem to be solved by the present invention is to provide a slag-forming agent containing rare earth oxides to address the shortcomings of the prior art, thereby achieving rapid slag formation, easy slag removal, no negative impact on the sulfur and phosphorus fixation performance of steel slag, and significant reduction in iron loss.

[0005] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:

[0006] A rare earth oxide-containing slag-forming agent, the main chemical components of which, by mass percentage, are REO: 7-23%, SiO2: 29-45%, Al2O3: 13-23%, CaO: 3-7%, MgO: 2-5%, Al: 0.5-1.5%, loss on ignition: 4-9%, and the remainder being unavoidable impurities.

[0007] Preferably, the REO is derived from rare earth mineral powder, and is at least one of La2O3, CeO2, Nd2O3 and Y2O3.

[0008] The above-mentioned rare earth oxide-containing slag-forming agent is composed of the following raw materials in parts by weight: 10-30 parts rare earth mineral powder, 40-60 parts lightly calcined perlite, 10-20 parts AD powder, and 10-20 parts dolomite powder.

[0009] Wherein: the rare earth mineral powder contains REO ≥ 70%, and REO is one or more of the components La2O3, CeO2, Nd2O3 and Y2O3.

[0010] The lightly calcined perlite is perlite ore heat-treated at 400℃-500℃, containing SiO2≥72%, Al2O3≥12%, and an expansion ratio≥10 (1350℃).

[0011] The AD powder contains elemental [Al] ≥ 5%, Al2O3 ≥ 75%, and S ≤ 0.2%.

[0012] The dolomite powder contains ≥30% CaO, ≥20% MgO, and has a loss on ignition ≥40%.

[0013] Preferably, the rare earth mineral powder has a mesh size of 100 mesh or more; the AD powder has a mesh size of 100 mesh or more; the dolomite powder has a mesh size of 150 mesh or more; and the lightly calcined perlite has a mesh size of 100 mesh or more.

[0014] Preferably, the rare earth mineral powder is one or a mixture of two types of fluorocarbon cerium ore powder and ionic rare earth mineral powder.

[0015] A method for preparing a rare earth oxide-containing slag-forming agent includes the following steps:

[0016] Ingredients: Raw materials are formulated according to the mass percentage of the rare earth oxide-containing slag-forming agent components mentioned above;

[0017] Mixing and grinding: Add the accurately measured materials to the mixing and grinding machine and mix and grind for 10-20 minutes to obtain a uniform mixture.

[0018] Drying: The above-mentioned uniformly mixed materials are put into a drying kiln for baking treatment. When the moisture content of the finished product is below 2%, it is cooled, packaged, and stored to obtain the finished product.

[0019] Preferably, the baking process conditions include: baking at 100-200℃ for 30-60 minutes.

[0020] The application method of the above-mentioned rare earth oxide-containing slag-forming agent in slag removal operation is as follows: determine the amount to be added according to the dosage of 0.3-0.6 kg / t of molten steel (iron); add the slag-forming agent directly to the slag surface, and mix the slag-forming agent with the steel slag by stirring with argon gas blown from the bottom of the ladle or by mechanical stirring with a slag remover. After 3-5 minutes, carry out the slag removal operation.

[0021] To address the aforementioned problems in existing technologies, metallurgists typically employ the addition of slag-forming agents. The raw materials for these agents are generally SiO2-containing materials such as crushed glass and perlite. Their working principle is as follows: after the slag-forming agent is added to the surface of molten steel, the lower layer of raw materials in direct contact with the molten steel melts upon heating and mixes with the existing steel slag, forming acidic "long slag" with reduced breakability; the upper layer of raw materials expands upon heating, agglomerating the steel slag into large slag blocks, facilitating slag removal. This method solves the problem of difficult slag removal. However, these slag-forming agents are purely acidic materials containing SiO2. Their addition to molten steel inevitably causes a significant decrease in the basicity of the steel slag, leading to problems such as "sulfurization" and "phosphorus reversion" in the slag, resulting in a decline in the quality of the molten steel.

[0022] Patent document CN112553409A discloses a vanadium-titanium ferroalloy slag-forming agent and its preparation method. The slag-forming agent comprises the following raw materials in parts by weight: 20-40 parts calcium oxide, 20-40 parts alumina, 10-30 parts porous silica, and 10-20 parts fibrous gypsum particles. The preparation method involves mixing the calcium oxide, alumina, porous silica, and fibrous gypsum particles according to the specified parts by weight, and drying until the moisture content is less than 2%, thus obtaining the slag-forming agent. The calcium oxide in the slag-forming agent increases the alkalinity of the desulfurization slag, promoting slag-iron separation and reducing iron loss; the porous silica and fibrous gypsum particles promote the aggregation of dilute slag, increasing the slag removal rate. This technical solution optimizes the overall performance of the slag-forming agent product. However, the following issues cannot be ignored: 1. The addition of 30-60 parts of calcium oxide and fibrous gypsum, while promoting slag agglomeration, will make the slag system alkaline, belonging to the "short slag" category of metallurgical slag systems. This results in a narrow solidification range and high fragmentation, which is not conducive to slag removal operations. 2. The fibrous gypsum used in the product contains [SiO4]. 2- Ions have a negative effect on the sulfur capacity of the slag system. During slag removal operations, the slag system's thermal conditions change due to the stirring caused by the slag remover, which poses a risk of "sulfur reversion" and "phosphorus reversion". 3. This technical solution achieves the goal of reducing iron loss mainly by promoting the separation of slag and iron interfaces, but the iron loss problem caused by the "iron encapsulation" phenomenon in the slag when slag lumps aggregate is not solved.

[0023] CN110117687A discloses a KR desulfurizing agent and a desulfurization method. The KR desulfurizing agent, by mass percentage, comprises the following components: 0 < aluminum ash ≤ 6%, lime ≥ 94%, and aluminum ash + lime: 100%. The chemical composition of the aluminum ash, by mass percentage, includes: Al: 20-25%, Al₂O₃: 30-40%, SiO₂: 5-10%, Na₂O: 2-3%, MgO: 2-3%, O < CaO < 2.00%, O < FeO + MnO < 1.0%. The desulfurization method using the KR desulfurizing agent includes the following steps: controlling the inlet temperature, inlet Si content, and inlet S content of the molten iron to be desulfurized; adding the KR desulfurizing agent to the molten iron to be desulfurized and performing KR stirring treatment; and after desulfurization is completed, performing slag removal treatment. The technology has the following shortcomings in actual production: 1. The desulfurization effect is based on nearly complete mass percentage of lime in the product, whose composition is CaO, to make the molten steel slag system in a high-alkalinity state to enhance the desulfurization effect; however, the high-alkalinity slag system is a brittle "short slag" recognized in the metallurgical industry, which will greatly increase the difficulty of slag removal operation; 2. The desulfurization product in this technical solution is CaS. (s) To reduce the difficulty of slag removal, it is necessary to add acidic slag-forming agents that are commonly used in the industry. However, this will reduce the alkalinity of the slag system, which will lead to a significant "sulfur reversion" problem.

[0024] Therefore, the applicant believes there is an urgent need for a slag-collecting agent product that is highly efficient, easy to collect, has no negative impact on the sulfur and phosphorus fixation properties of steel slag, and can significantly reduce iron loss.

[0025] The slag agglomerator of this invention uses perlite, one of its raw materials, which is widely available and inexpensive. Upon heating, perlite rapidly expands in volume, producing an excellent effect of agglomerating slag lumps. Rare earth mineral powder, another raw material, contains REO, an excellent desulfurization and dephosphorization carrier. It can combine with sulfur in the slag to form RE2O2S-type rare earth sulfur compounds and RE2O5P-type rare earth phosphorus compounds with melting points above 2000℃. These compounds can stably exist in steel slag, offsetting the "sulfur reversion" and "phosphorus reversion" problems in molten steel caused by the reduction in slag basicity due to the addition of the slag agglomerator. Furthermore, it can react with Al2O3 in the steel slag to form xREO.yAl2O3 compounds, reducing the activity of Al2O3 in the steel slag and increasing the adsorption effect of the steel slag on inclusions in the molten steel. One of the raw materials used, AD powder, contains a certain proportion of elemental [Al], which can undergo an exothermic redox reaction with oxides in steel slag, optimizing the thermodynamic environment of the slag interface and promoting the mixing reaction between slag components. The Al2O3 component it contains can increase the viscosity of the steel slag and promote slag agglomeration. Another raw material used, dolomite, contains CaCO3 and MgCO3, which can decompose into CaO and MgO at 750℃-950℃, serving as excellent carriers for sulfur and phosphorus fixation. More importantly, the CO2 gas released during decomposition can thoroughly stir the interior of the steel slag, fundamentally breaking down the "iron-coated" small areas within the slag, allowing the molten steel (iron) droplets to fall back into the molten steel under their own gravity, directly improving metal recovery and reducing iron loss. Furthermore, the specific amounts of MgO and Al2O3 in the slag agglomerator product of this invention are the most effective components for increasing the interfacial tension between steel and slag, achieving good steel-slag separation during slag removal and reducing iron loss.

[0026] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0027] 1. By utilizing rare earth oxides and controlling the REO mass percentage between 7-23%, the rare earth oxides are derived from rare earth minerals and are at least one of La2O3, CeO2, Nd2O3 and Y2O3, which greatly increases the sulfur capacity in the slag and enhances the sulfur fixation and phosphorus fixation effects.

[0028] 2. To increase the viscosity of steel slag, an appropriate amount of AD powder is added to the product to introduce Al2O3, which facilitates slag removal. At the same time, the addition of rare earth elements can suppress the problem of reduced sulfur and phosphorus solidification effect caused by the increase of Al2O3 content.

[0029] 3. AD powder contains a small amount of elemental aluminum, which can react with Fe in the slag. 2+ Fe 3+Si 2+ Further reactions not only increase metal recovery rate, but also optimize the thermodynamic and dynamic environment of the slag interface due to the exothermic nature of the aluminothermic reaction, thus further promoting slag aggregation.

[0030] 4. Adding a certain proportion of CaCO3 and MgCO3 has several benefits. First, when heated, they release CO2 gas, which has a micro-stirring effect on the slag interface and breaks the "iron coating" phenomenon. Second, the decomposed residues CaO and MgO are excellent carriers for sulfur and phosphorus fixation. MgO can also increase the interfacial tension between steel and slag, promoting the separation of steel and slag during the slag removal process.

[0031] 5. The main raw material of this slag-forming agent is perlite containing SiO2, which is widely available, inexpensive, and easy to control in terms of cost. Detailed Implementation

[0032] To better understand the present invention, the following embodiments further illustrate the content of the invention, but the scope of protection of the present invention is not limited to the following embodiments. Numerous specific details are set forth in the following description to provide a more thorough understanding of the invention. However, it will be apparent to those skilled in the art that the present invention can be practiced without one or more of these details.

[0033] In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values.

[0034] Unless otherwise specified, all raw materials are derived from commercially available products and do not contain any unspecified components other than unavoidable impurities.

[0035] In this invention, unless otherwise specified, numbers with % refer to mass fractions.

[0036] This invention provides a rare earth oxide-containing slag-forming agent, prepared using materials containing REO, SiO2, Al2O3, CaO, MgO, and Al, wherein:

[0037] REO is derived from rare earth mineral powder, which contains ≥70% REO. REO is at least one of La2O3, CeO2, Nd2O3, and Y2O3. When REO is a combination of two or more of the components La2O3, CeO2, Nd2O3, and Y2O3, there is no particular restriction on the content ratio of La2O3, CeO2, Nd2O3, and Y2O3.

[0038] The rare earth mineral powder is selected from one or a mixture of fluorocarbon cerium ore powder and ion-adsorption rare earth mineral powder; when the rare earth mineral powder is selected from a mixture of fluorocarbon cerium ore powder and ion-adsorption rare earth mineral powder, the weight ratio of the two is not particularly limited and can be selected as (0.1%-99.9%):(0.1%-99.9%).

[0039] Lightly calcined perlite is perlite ore heat-treated at 400℃-500℃, containing SiO2≥72%, Al2O3≥12%, and an expansion ratio≥10 at 1350℃.

[0040] AD powder contains elemental [Al] ≥ 5%, Al2O3 ≥ 75%, and S ≤ 0.2%;

[0041] The dolomite powder contains ≥30% CaO, ≥20% MgO, and has a loss on ignition ≥40%.

[0042] Rare earth mineral powder has a mesh size of 100 mesh or higher; AD powder has a mesh size of 100 mesh or higher; dolomite powder has a mesh size of 150 mesh or higher; and lightly calcined perlite has a mesh size of 100 mesh or higher.

[0043] The following are specific implementation case examples:

[0044] Example 1

[0045] A rare earth oxide-containing slag-forming agent, whose main chemical components, by mass percentage, are REO: 7.0%, SiO2: 45.0%, Al2O3: 18.5%, CaO: 4.5%, MgO: 4.5%, Al: 0.8%, loss on ignition: 6.0%, with the remainder being unavoidable impurities; raw materials are prepared according to the above mass percentages; then, by weight, 10 parts of rare earth mineral powder, 60 parts of lightly calcined perlite, 15 parts of AD powder, and 15 parts of dolomite powder are provided. The above materials are mixed and added to a mixing mill, and mixed for 10 minutes to obtain a uniformly mixed material; the uniformly mixed material is then fed into a drying kiln and baked at 200℃ for 30 minutes. When the finished product has a moisture content of less than 2%, it is cooled, packaged, and stored to obtain the finished product.

[0046] In this embodiment, the rare earth mineral powder is selected from fluorocarbon cerium ore powder, and the composition contains REO ≥ 70%, wherein REO is La2O3 and CeO2;

[0047] Lightly calcined perlite is perlite ore heat-treated at 400℃, containing SiO2≥72%, Al2O3≥12%, and an expansion ratio≥10 (1350℃);

[0048] AD powder contains elemental [Al] ≥ 5%, Al2O3 ≥ 75%, and S ≤ 0.2%;

[0049] The dolomite powder contains ≥30% CaO, ≥20% MgO, and has a loss on ignition ≥40%.

[0050] The rare earth mineral powder has a mesh size of 100; the AD powder has a mesh size of 100; the dolomite powder has a mesh size of 150; and the lightly calcined perlite has a mesh size of 100.

[0051] Example 2

[0052] A rare earth oxide-containing slag-forming agent, whose main chemical components, by mass percentage, are REO: 9.2%, SiO2: 34.0%, Al2O3: 20.8%, CaO: 6.0%, MgO: 4.0%, Al: 1.2%, loss on ignition: 8.2%, with the remainder being unavoidable impurities; raw materials are prepared according to the above mass percentages; then, by weight, 13 parts of rare earth mineral powder, 47 parts of lightly calcined perlite, 20 parts of AD powder, and 20 parts of dolomite powder are provided. The above materials are mixed and added to a mixing mill, and mixed for 20 minutes to obtain a uniformly mixed material; the uniformly mixed material is then fed into a drying kiln and baked at 180°C for 40 minutes. When the finished product has a moisture content of less than 2%, it is cooled, packaged, and stored to obtain the finished product.

[0053] In this embodiment, the rare earth mineral powder is selected from a mixture of fluorocarbon cerium ore powder and ion-adsorption rare earth mineral powder, and the composition contains REO ≥ 70%, wherein REO is La2O3, CeO2, Nd2O3 and Y2O3;

[0054] Lightly calcined perlite is perlite ore heat-treated at 450℃, containing SiO2≥72%, Al2O3≥12%, and an expansion ratio≥10 (1350℃);

[0055] AD powder contains elemental [Al] ≥ 5%, Al2O3 ≥ 75%, and S ≤ 0.2%;

[0056] The dolomite powder contains ≥30% CaO, ≥20% MgO, and has a loss on ignition ≥40%.

[0057] The rare earth mineral powder has a mesh size of 100; the AD powder has a mesh size of 100; the dolomite powder has a mesh size of 150; and the lightly calcined perlite has a mesh size of 100.

[0058] Example 3

[0059] A rare earth oxide-containing slag-forming agent, whose main chemical components, by mass percentage, are REO: 13.1%, SiO2: 38.3%, Al2O3: 14.3%, CaO: 5.8%, MgO: 3.9%, Al: 0.6%, loss on ignition: 7.7%, with the remainder being unavoidable impurities; raw materials are prepared according to the above mass percentages; then, by weight, 18 parts of rare earth mineral powder, 53 parts of lightly calcined perlite, 10 parts of AD powder, and 19 parts of dolomite powder are provided. The above materials are mixed and added to a mixing mill, and mixed for 18 minutes to obtain a uniformly mixed material; the uniformly mixed material is then fed into a drying kiln and baked at 125°C for 50 minutes. When the moisture content of the finished product is below 2%, it is cooled, packaged, and stored to obtain the finished product.

[0060] In this embodiment, the rare earth mineral powder is selected from a mixture of fluorocarbon cerium ore powder and ion-adsorption rare earth mineral powder, and the composition contains REO ≥ 70%, wherein REO is La2O3, CeO2, Nd2O3 and Y2O3;

[0061] Lightly calcined perlite is perlite ore heat-treated at 500℃, containing SiO2≥72%, Al2O3≥12%, and an expansion ratio≥10 (1350℃);

[0062] AD powder contains elemental [Al] ≥ 5%, Al2O3 ≥ 75%, and S ≤ 0.2%;

[0063] The dolomite powder contains ≥30% CaO, ≥20% MgO, and has a loss on ignition ≥40%.

[0064] The rare earth mineral powder has a mesh size of 100; the AD powder has a mesh size of 100; the dolomite powder has a mesh size of 150; and the lightly calcined perlite has a mesh size of 100.

[0065] Example 4

[0066] A rare earth oxide-containing slag-forming agent, whose main chemical components, by mass percentage, are REO: 14.8%, SiO2: 40.3%, Al2O3: 15.8%, CaO: 3.6%, MgO: 2.4%, Al: 0.6%, loss on ignition: 4.8%, with the remainder being unavoidable impurities; raw materials are prepared according to the above mass percentages; then, by weight, 20 parts of rare earth mineral powder, 56 parts of lightly calcined perlite, 12 parts of AD powder, and 12 parts of dolomite powder are provided. The above materials are mixed and added to a mixing mill, and mixed for 10 minutes to obtain a uniformly mixed material; the uniformly mixed material is then fed into a drying kiln and baked at 200℃ for 30 minutes. When the moisture content of the finished product is below 2%, it is cooled, packaged, and stored to obtain the finished product.

[0067] In this embodiment, the rare earth mineral powder is selected from a mixture of fluorocarbon cerium ore powder and ion-adsorption rare earth mineral powder, and the composition contains REO ≥ 70%, wherein REO is La2O3, CeO2, Nd2O3 and Y2O3;

[0068] Lightly calcined perlite is perlite ore heat-treated at 450℃, containing SiO2≥72%, Al2O3≥12%, and an expansion ratio≥10 (1350℃);

[0069] AD powder contains elemental [Al] ≥ 5%, Al2O3 ≥ 75%, and S ≤ 0.2%;

[0070] The dolomite powder contains ≥30% CaO, ≥20% MgO, and has a loss on ignition ≥40%.

[0071] The rare earth mineral powder has a mesh size of 200; the AD powder has a mesh size of 200; the dolomite powder has a mesh size of 200; and the lightly calcined perlite has a mesh size of 200.

[0072] Example 5

[0073] A rare earth oxide-containing slag-forming agent, whose main chemical components, by mass percentage, are REO: 20.7%, SiO2: 33.2%, Al2O3: 18.3%, CaO: 3.1%, MgO: 2.0%, Al: 1.0%, loss on ignition: 4.0%, with the remainder being unavoidable impurities; raw materials are prepared according to the above mass percentages; then, by weight, 28 parts of rare earth mineral powder, 45 parts of lightly calcined perlite, 17 parts of AD powder, and 10 parts of dolomite powder are provided. The above materials are mixed and added to a mixing mill, and mixed for 20 minutes to obtain a uniformly mixed material; the uniformly mixed material is then fed into a drying kiln and baked at 100°C for 60 minutes. When the finished product has a moisture content of less than 2%, it is cooled, packaged, and stored to obtain the finished product.

[0074] In this embodiment, the rare earth mineral powder is selected from a mixture of fluorocarbon cerium ore powder and ion-adsorption rare earth mineral powder, and the composition contains REO ≥ 70%, wherein REO is La2O3, CeO2, Nd2O3 and Y2O3;

[0075] Lightly calcined perlite is perlite ore heat-treated at 450℃, containing SiO2≥72%, Al2O3≥12%, and an expansion ratio≥10 (1350℃);

[0076] AD powder contains elemental [Al] ≥ 5%, Al2O3 ≥ 75%, and S ≤ 0.2%;

[0077] The dolomite powder contains ≥30% CaO, ≥20% MgO, and has a loss on ignition ≥40%.

[0078] The rare earth mineral powder has a mesh size of 300; the AD powder has a mesh size of 300; the dolomite powder has a mesh size of 300; and the lightly calcined perlite has a mesh size of 300.

[0079] Example 6

[0080] A rare earth oxide-containing slag-forming agent, whose main chemical components, by mass percentage, are REO: 21.2%, SiO2: 29.1%, Al2O3: 19.1%, CaO: 3.3%, MgO: 2.2%, Al: 1.3%, loss on ignition: 6.4%, with the remainder being unavoidable impurities; raw materials are prepared according to the above mass percentages; then, by weight, 30 parts of rare earth mineral powder, 40 parts of lightly calcined perlite, 19 parts of AD powder, and 11 parts of dolomite powder are provided. The above materials are mixed and added to a mixing mill, and mixed for 15 minutes to obtain a uniformly mixed material; the uniformly mixed material is then fed into a drying kiln and baked at 150°C for 45 minutes. When the moisture content of the finished product is below 2%, it is cooled, packaged, and stored to obtain the finished product.

[0081] In this embodiment, the rare earth mineral powder is selected from a mixture of fluorocarbon cerium ore powder and ion-adsorption rare earth mineral powder, and the composition contains REO ≥ 70%, wherein REO is La2O3, CeO2, Nd2O3 and Y2O3;

[0082] Lightly calcined perlite is perlite ore heat-treated at 450℃, containing SiO2≥72%, Al2O3≥12%, and an expansion ratio≥10 (1350℃);

[0083] AD powder contains elemental [Al] ≥ 5%, Al2O3 ≥ 75%, and S ≤ 0.2%;

[0084] The dolomite powder contains ≥30% CaO, ≥20% MgO, and has a loss on ignition ≥40%.

[0085] The rare earth mineral powder has a mesh size of 100; the AD powder has a mesh size of 100; the dolomite powder has a mesh size of 150; and the lightly calcined perlite has a mesh size of 100.

[0086] Instructions for use: The above-mentioned slag-coagulating agent is applied in slag removal operations. The specific method of use is as follows: determine the amount of slag-coagulating agent to be added according to the dosage of 0.3-0.6 kg / t of molten steel (iron); add the slag-coagulating agent directly to the slag surface, and mix the slag-coagulating agent with the steel slag by stirring with argon gas blown from the bottom of the ladle or by mechanical stirring with a slag remover. After 3-5 minutes, carry out the slag removal operation.

[0087] The following are comparative case studies:

[0088] Comparative Example 1

[0089] The difference between Comparative Example 1 and Example 1 is that the slag-forming agent does not contain REO, and the corresponding rare earth minerals are omitted from the preparation materials. Specifically:

[0090] A slag-forming agent, whose main chemical components, by mass percentage, are SiO2: 46.8%, Al2O3: 19.05%, CaO: 6.0%, MgO: 4.0%, Al: 0.75%, loss on ignition: 8.0%, with the remainder being unavoidable impurities; raw materials are prepared according to the above mass percentages; then, by weight, 65 parts of lightly calcined perlite, 15 parts of AD powder, and 20 parts of dolomite powder are provided. The above materials are mixed and added to a mixing mill, and mixed for 10 minutes to obtain a uniformly mixed material; the uniformly mixed material is then fed into a drying kiln and baked at 200°C for 30 minutes. When the moisture content of the finished product is below 2%, it is cooled, packaged, and stored to obtain the finished product.

[0091] Comparative Example 2

[0092] The difference between Comparative Example 2 and Example 1 is that the slag-forming agent does not contain Al, and AD powder is omitted from the corresponding preparation materials. Specifically:

[0093] A slag-forming agent, whose main chemical components, by mass percentage, are REO: 7.0%, SiO2: 43.2%, Al2O3: 7.2%, CaO: 9.0%, MgO: 6.0%, loss on ignition: 12.2%, with the remainder being unavoidable impurities; raw materials are prepared according to the above mass percentages; then, by weight, 10 parts rare earth mineral powder, 60 parts lightly calcined perlite, and 30 parts dolomite powder are provided. The above materials are mixed and added to a mixing mill, and mixed for 10 minutes to obtain a uniformly mixed material; the uniformly mixed material is then fed into a drying kiln and baked at 200°C for 30 minutes. When the moisture content of the finished product is below 2%, it is cooled, packaged, and stored to obtain the finished product.

[0094] Comparative Example 3

[0095] A slag-forming agent (refer to Example 1 disclosed in CN104894324A) has the following chemical composition by mass percentage: 65% SiO2, 18% CaCO3, 14% MgCO3, and 3% Al2O3.

[0096] Comparative Example 4

[0097] A slag-forming agent (refer to Example 1 disclosed in CN110317925A) is composed of the following components in mass percentage: 30 wt% CaO, 30 wt% SiC, 15 wt% Fe2O3, 10 wt% MgO, and 15 wt% yttrium-based rare earth alloy; each component is weighed according to the formula and added to a mixing device, and mixed by centrifugal mixing for 20 min.

[0098] Comparative Example 5

[0099] A slag-forming agent (refer to Example 1 disclosed in CN110117687A) comprises, by weight percentage, the following components: 6% aluminum ash and 94% lime. The chemical composition of the aluminum ash, by weight percentage, includes: Al: 25%, Al₂O₃: 40%, SiO₂: 10%, Na₂O: 3%, MgO: 3%, CaO: 2.00%, FeO+MnO: 1.0%. The lime, by weight percentage, contains 95% CaO.

[0100] Next, the content of the evaluation experiment will be explained.

[0101] The slag-reducing agents prepared in Examples 1-3 and Comparative Examples 1-5 were used in the slag removal operation of a steel plant. The amount of slag-reducing agent added was determined according to the dosage of 0.5 kg / t of molten steel (iron). The slag-reducing agent was directly added to the slag surface, and the slag-reducing agent and steel slag were mixed by stirring with argon gas blown from the bottom of the ladle. The slag removal operation was carried out 5 minutes later.

[0102] The following evaluation criteria should be completed during the use of the slag-forming agent:

[0103] (1) Measure and record the sulfur content in the molten iron before and after the slag removal of the slag-collecting agent;

[0104] (2) Record the slag removal time and amount, and calculate the slag removal efficiency;

[0105] (3) Measure and record iron loss.

[0106] The measurement results are shown in the table below:

[0107]

[0108] The above results show that the slag-forming agent of the present invention has a good sulfur-fixing effect and is not prone to "sulfur reversion" problems; the slag removal rate is as high as 85% or more, indicating that the slag is formed quickly and the slag lumps are easy to remove; at the same time, it can also significantly reduce iron loss. Compared with the existing methods, the reduction in iron loss is more than 50%, showing significant progress overall.

[0109] Furthermore, those skilled in the art should understand that although many problems exist in the prior art, each embodiment or technical solution of the present invention can be improved in only one or a few aspects, without necessarily solving all the technical problems listed in the prior art or the background art simultaneously. Those skilled in the art should understand that any content not mentioned in a claim should not be construed as a limitation on that claim.

[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Any other modifications or equivalent substitutions made by those skilled in the art to the technical solutions of the present invention, as long as they do not depart from the spirit and scope of the technical solutions of the present invention, should be covered within the scope of the claims of the present invention.

Claims

1. A slag-forming agent containing rare earth oxides, characterized in that: Its main chemical composition, by mass percentage, is REO: 7-23%, SiO2: 29-45%, Al2O3: 13-23%, CaO: 3-7%, MgO: 2-5%, Al: 0.5-1.5%, loss on ignition: 4-9%, with the remainder being unavoidable impurities; the REO is derived from rare earth mineral powder, and is at least one of La2O3, CeO2, Nd2O3, and Y2O3; the raw materials of the slag agglomerator, by weight, are: rare earth mineral powder 10-30 parts, lightly calcined perlite 40-60 parts, AD powder 10-20 parts, dolomite powder 1 0-20 parts; the rare earth mineral powder contains REO ≥ 70%, and REO is one or more of La2O3, CeO2, Nd2O3 and Y2O3; the lightly calcined perlite is perlite ore heat-treated at 400℃-500℃, containing SiO2 ≥ 72%, Al2O3 ≥ 12%, and an expansion ratio of ≥ 10 at 1350℃; the AD powder contains elemental [Al] ≥ 5%, Al2O3 ≥ 75%, and S ≤ 0.2%; the dolomite powder contains CaO ≥ 30%, MgO ≥ 20%, and a loss on ignition ≥ 40%.

2. The slag-forming agent containing rare earth oxides as described in claim 1, characterized in that: The rare earth mineral powder has a mesh size of 100 mesh or higher; the AD powder has a mesh size of 100 mesh or higher; the dolomite powder has a mesh size of 150 mesh or higher; and the lightly calcined perlite has a mesh size of 100 mesh or higher.

3. The slag-forming agent containing rare earth oxides as described in claim 1, characterized in that: The rare earth mineral powder is one or a mixture of two types of fluorocarbon cerium ore powder and ionic rare earth mineral powder.

4. A method for preparing a rare earth oxide-containing slag-forming agent as described in any one of claims 1-3, characterized in that: Includes the following steps: Ingredients: Raw materials are formulated according to the mass percentage of the rare earth oxide-containing slag-forming agent components mentioned above; Mixing and grinding: Add the accurately measured materials to the mixing and grinding machine and mix and grind for 10-20 minutes to obtain a uniform mixture. Drying: The above-mentioned uniformly mixed materials are put into a drying kiln for baking treatment. When the moisture content of the finished product is below 2%, it is cooled, packaged, and stored to obtain the finished product.

5. The method for preparing a rare earth oxide-containing slag-forming agent as described in claim 4, characterized in that: The baking process conditions include: baking at 100-200℃ for 30-60 minutes.

6. The application of the slag-collecting agent as described in any one of claims 1-3 or the slag-collecting agent obtained by the preparation method as described in claim 4 or 5 in slag removal operations.

7. The application of the slag-collecting agent as described in claim 6 in slag removal operations, characterized in that: The method of use is as follows: determine the amount of slag-coagulating agent to be added according to the dosage of 0.3-0.6 kg / t of molten steel; add the slag-coagulating agent directly to the slag surface, and mix the slag-coagulating agent with the steel slag by stirring with argon gas blown from the bottom of the ladle or by mechanical stirring with a slag remover. After 3-5 minutes, carry out the slag removal operation.

Citation Information

Patent Citations

  • KR desulfurizing agent and desulfurizing method

    CN110117687A

  • Molten steel purifying agent for cast steel roller and preparing method and using method

    CN110317925A

  • Vanadium-titanium-containing molten iron slag accretion agent and preparation method thereof

    CN112553409A

  • Slag conglomeration agent for reducing slag removal iron loss of molten iron pretreatment, and use method thereof

    CN104894324A

  • Electroslag remelting slag system for duplex stainless steel