Three-dimensional graphene-reinforced copper-based composite material, preparation method and application thereof
Three-dimensional graphene was grown in situ on the surface of copper foam by chemical vapor deposition and hot pressing sintering technology, which solved the problem of graphene agglomeration and prepared a high-strength, high-conductivity three-dimensional graphene-reinforced copper-based composite material, improving the mechanical and electrical properties of the material.
Patent Information
- Application Number
- CN202311590236.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-27
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-11-27
AI Technical Summary
In the preparation of three-dimensional graphene-reinforced copper-based composite materials, existing technologies have shown that graphene is prone to agglomeration, which leads to a decrease in mechanical properties and material plasticity, and the continuity and uniformity of graphene are difficult to control.
Three-dimensional graphene was grown in situ on the surface of copper foam using chemical vapor deposition. By controlling the process parameters, a highly continuous three-dimensional graphene network was constructed. Combined with hot pressing sintering technology, a composite material with high strength and high conductivity was prepared.
The uniformity and continuity of graphene in copper-based composite materials were achieved, which improved the mechanical and electrical properties of the materials, reduced adhesive wear, and enhanced the wear resistance of the materials.
Smart Images

Figure CN117604491B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal matrix composites, and more particularly to a three-dimensional graphene-reinforced copper matrix composite material, its preparation method, and its applications. Background Technology
[0002] Copper is a traditional metallic material with excellent electrical and thermal conductivity, widely used in electronic devices, transportation, and aerospace. However, in today's rapidly evolving technological landscape, copper's poor heat and corrosion resistance makes it difficult to meet industrial demands, thus necessitating the development of new materials. Graphene-reinforced copper-based composites are a novel material with excellent comprehensive properties. Thanks to the large number of free electrons within the graphene sheets, high-speed pathways for charge carriers are formed in the copper-based composite, enhancing current transmission and resulting in superior electrical conductivity. However, conventional mechanical mixing of copper powder and graphene introduces numerous defects into the graphene, and the van der Waals forces between graphene sheets make two-dimensional graphene prone to aggregation, leading to a significant decrease in mechanical properties and material plasticity.
[0003] Three-dimensional graphene networks are a novel structure that can effectively solve the problem of graphene agglomeration. Currently, methods for preparing three-dimensional graphene-reinforced copper-based composites can be broadly divided into two categories: one is the graphene framework-filling method, which uses graphene foam frameworks as fillers. This method causes significant damage to the graphene, resulting in poor structural stability and a complex process. The other is the powder surface deposition method, which grows or adsorbs graphene in situ on the surface of copper powder, followed by sintering for densification. However, the continuity of the graphene prepared by this method is questionable, and controlling the uniformity of graphene on the copper powder surface is also a major challenge. Summary of the Invention
[0004] The purpose of this invention is to provide a three-dimensional graphene-reinforced copper-based composite material, its preparation method, and its applications. In the preparation method provided by this invention, graphene exhibits three-dimensional continuity and high reinforcement efficiency, resulting in a three-dimensional graphene-reinforced composite material with high strength and high electrical conductivity.
[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0006] This invention provides a method for preparing a three-dimensional graphene-reinforced copper-based composite material, comprising the following steps:
[0007] (1) Place the foamed copper into a chemical vapor deposition tube furnace, introduce reducing gas and protective gas, raise the temperature, and anneal to remove the surface oxide layer and impurities to obtain pretreated foamed copper.
[0008] (2) Add a carbon source to deposit and grow three-dimensional graphene in situ on the pretreated copper foam obtained in step (1);
[0009] (3) Deplete or turn off the carbon source in step (2), cool to room temperature, and obtain copper foam supported graphene;
[0010] (4) Densify the copper-supported graphene foam obtained in step (3) to obtain a three-dimensional graphene-reinforced copper-based composite material.
[0011] Preferably, the porosity of the copper foam in step (1) is 10 to 150 PPI.
[0012] Preferably, the reducing gas in step (1) is H2, the protective gas is Ar, the flow rate ratio of the reducing gas to the protective gas is (1-100):300, and the total flow rate of the reducing gas and the protective gas is 1-1200 sccm.
[0013] Preferably, the annealing temperature in step (1) is 500-1050°C and the annealing time is 0-12h.
[0014] Preferably, the growth temperature of the three-dimensional graphene in step (2) is 800-1050℃ and the growth time is 0-5h.
[0015] Preferably, the carbon source in step (2) includes a gaseous carbon source, a liquid carbon source, or a solid carbon source.
[0016] Preferably, the densification method in step (4) is hot pressing sintering.
[0017] Preferably, the densification temperature in step (4) is 800-1000℃, the heating rate is 10-20℃ / min, the holding time is 0.5-2h, the pressure is 20-50MPa, and the cooling method is furnace cooling.
[0018] This invention provides a three-dimensional graphene-reinforced copper-based composite material prepared by the preparation method described in the above technical solution.
[0019] The present invention also provides the application of the three-dimensional graphene-reinforced copper-based composite material described above in electronic and electrical equipment and power transmission.
[0020] This invention provides a method for preparing a three-dimensional graphene-reinforced copper-based composite material, comprising the following steps: (1) placing copper foam in a chemical vapor deposition tube furnace, introducing reducing gas and protective gas, raising the temperature, and annealing to remove the surface oxide layer and impurities to obtain pretreated copper foam; (2) adding a carbon source to deposit and grow three-dimensional graphene on the surface of the pretreated copper foam obtained in step (1); (3) depleting or turning off the carbon source in step (2), cooling to room temperature to obtain copper foam loaded with graphene; (4) densifying the copper foam loaded with graphene obtained in step (3) to obtain a three-dimensional graphene-reinforced copper-based composite material. This invention utilizes chemical vapor deposition to deposit graphene in situ on the surface of copper foam, constructing an ideal three-dimensional graphene network structure. Compared with powder sintering, the graphene exhibits higher uniformity and continuity. By controlling the chemical vapor deposition process, the controllability of the number of graphene layers and defect density is enhanced. The resulting composite material has a lower graphene content and higher reinforcement efficiency. After hot pressing and sintering, a three-dimensional graphene-reinforced copper-based composite material with excellent physical and mechanical properties can be obtained. Attached Figure Description
[0021] Figure 1 The images are SEM images of copper-supported graphene foam prepared in step (2) of Example 2 of this invention at different magnifications. Detailed Implementation
[0022] This invention provides a method for preparing a three-dimensional graphene-reinforced copper-based composite material, comprising the following steps:
[0023] (1) Place the foamed copper into a chemical vapor deposition tube furnace, introduce reducing gas and protective gas, raise the temperature, and anneal to remove the surface oxide layer and impurities to obtain pretreated foamed copper.
[0024] (2) Add a carbon source to deposit and grow three-dimensional graphene in situ on the pretreated copper foam obtained in step (1);
[0025] (3) Deplete or turn off the carbon source in step (2), cool to room temperature, and obtain copper foam supported graphene;
[0026] (4) Densify the copper-supported graphene foam obtained in step (3) to obtain a three-dimensional graphene-reinforced copper-based composite material.
[0027] Unless otherwise specified, the present invention does not have any special limitations on the source of the raw materials, and commercially available products well known to those skilled in the art can be used.
[0028] This invention involves placing copper foam into a chemical vapor deposition tube furnace, introducing reducing and protective gases, raising the temperature, and annealing to remove the surface oxide layer and impurities, thereby obtaining pretreated copper foam.
[0029] In this invention, the porosity of the copper foam is preferably 10–150 PPI, more preferably 60–120 PPI, and most preferably 95 PPI. In this invention, the copper foam has a high porosity, exceeding 98%, resulting in more uniform graphene growth and further improving the performance of the composite material.
[0030] In this invention, the reducing gas is preferably H2; the protective gas is preferably Ar; the flow rate ratio of the reducing gas to the protective gas is preferably (1-100):300; and the total flow rate of the reducing gas and the protective gas is preferably 1-1200 sccm.
[0031] In this invention, the annealing temperature is preferably 500–1050°C; the annealing time is preferably 0–12 h. The annealing process of this invention can effectively remove the oxide layer and impurities from the surface of the copper foam, which is beneficial for the quality control of graphene.
[0032] After obtaining pretreated foamed copper, the present invention adds a carbon source to deposit and grow three-dimensional graphene in situ on the surface of the pretreated foamed copper.
[0033] In this invention, the carbon source preferably includes a gaseous carbon source, a liquid carbon source, or a solid carbon source.
[0034] This invention adjusts the addition method according to the type of carbon source. In this invention, when the carbon source is a solid carbon source, it is preferable to mix the solid carbon source and a solvent to obtain a solid carbon source solution, then immerse the pretreated copper foam in the solid carbon source solution, dry it, and then heat it to the graphene growth temperature to deposit and grow three-dimensional graphene in situ on the surface of the pretreated copper foam.
[0035] In this invention, the solid carbon source preferably includes a carbon-containing polymer, more preferably polymethyl methacrylate.
[0036] In this invention, the solvent preferably includes one of N,N-dimethylformamide, toluene, tetrahydrofuran, and chloroform.
[0037] In this invention, the concentration of the solid carbon source solution is preferably 1-500 mg / mL, more preferably 5-400 mg / mL, and most preferably 5-200 mg / mL.
[0038] In this invention, the impregnation temperature is preferably 40–70°C, more preferably 50–60°C; the impregnation time is preferably 10–30 min, more preferably 15–20 min; and the impregnation is preferably performed under ultrasonic conditions. This invention does not have a specific limitation on the ultrasonic power; any ultrasonic power well-known to those skilled in the art can be used. This invention does not have a specific limitation on the amount of the solid carbon source solution used; it only needs to be sufficient to submerge the copper foam. By limiting the impregnation temperature and time to the above ranges, this invention can more effectively remove air from the pores of the copper foam, allowing the solid carbon source to be more fully impregnated into the copper foam.
[0039] In this invention, the drying temperature is preferably 60-80°C, more preferably 70°C; the drying time is preferably 10-14 hours, more preferably 12 hours.
[0040] In this invention, when the carbon source is a gaseous carbon source, it is preferable to first heat the material to the graphene growth temperature and then introduce the gaseous carbon source. In this invention, the flow rate of the gaseous carbon source is preferably 2–50 sccm.
[0041] In this invention, the gaseous carbon source preferably includes CH4, C2H2 or C3H3.
[0042] In this invention, when the carbon source is a liquid carbon source, the liquid carbon source is preferably anhydrous ethanol.
[0043] In this invention, when the liquid carbon source is anhydrous ethanol, it is preferable to evaporate the anhydrous ethanol and, after the furnace reaches the graphene growth temperature, open the ethanol gas channel and introduce it into the chemical vapor deposition tube furnace along with the protective gas Ar.
[0044] In this invention, the amount of liquid carbon source added is preferably 1 to 10 ml.
[0045] In this invention, the growth temperature of the three-dimensional graphene is preferably 800–1050°C, more preferably 1000°C; the growth time is preferably 0–5 h, more preferably 30 min. The chemical vapor deposition method used in this invention is beneficial for improving the quality of graphene, controlling the number of graphene layers and defect density, and thus constructing an ideal three-dimensional graphene network.
[0046] In this invention, reducing gas and protective gas are continuously introduced during the growth of the three-dimensional graphene.
[0047] In this invention, during the graphene deposition process, the carbon source is cracked to generate graphene.
[0048] After growth is complete, the carbon source is depleted or turned off, and the material is cooled to room temperature to obtain copper foam-supported graphene.
[0049] In this invention, when the carbon source is a gaseous carbon source, it is preferable to shut off the gaseous carbon source inflow; when the carbon source is a solid carbon source or a liquid carbon source, it is preferable to deplete the solid carbon source or the liquid carbon source.
[0050] In this invention, reducing gas and protective gas are continuously introduced during the cooling process.
[0051] In this invention, during the cooling process, the flow ratio of reducing gas to protective gas is preferably (1-100):300, and the total flow rate of reducing gas and protective gas is preferably 1-1200 sccm.
[0052] In this invention, the preferred cooling method is to rapidly cool down by cutting open the furnace body or to cool down with the furnace, more preferably by rapidly cooling down by cutting open the furnace body. In this invention, rapid cooling prevents graphene from developing excessive wrinkles and detaching from the surface of the copper foam during the cooling process due to the difference in thermal expansion coefficients between graphene and copper foam.
[0053] After obtaining copper-supported graphene foam, the present invention densifies the copper-supported graphene foam to obtain a copper-based graphene composite material.
[0054] In this invention, densification is preferably achieved through hot pressing and sintering.
[0055] In this invention, the hot pressing sintering process preferably includes: heating to the holding temperature and pressure of hot pressing sintering in one step or heating to the holding temperature and pressure of hot pressing sintering in stages.
[0056] In this invention, the densification temperature for the first heating to hot pressing sintering is preferably 800-1000℃, more preferably 900℃, the heating rate is preferably 10-20℃ / min, the holding time is preferably 0.5-2h, more preferably 1h, and the densification pressure is preferably 20-50MPa, more preferably 40MPa.
[0057] In this invention, the preferred holding temperature and pressure for the staged heating to hot pressing sintering are: first, heating to 650-750°C and pressure to 15-25 MPa, then heating to 780-820°C and pressure to 28-32 MPa, and finally heating to 800-1000°C and pressure to 35-50 MPa.
[0058] In this invention, the hot-pressing sintering can compact the foamed copper matrix to obtain a dense composite material. By limiting the temperature, time, and other parameters of the hot-pressing sintering to the aforementioned ranges, this invention can improve the density of the composite material and further enhance its performance.
[0059] After hot pressing and sintering, the present invention preferably cools the hot pressing and sintering product to obtain a three-dimensional graphene-reinforced copper-based composite material.
[0060] This invention constructs a three-dimensional continuous graphene network structure within a copper matrix by hot-pressing and sintering graphene-loaded copper foam. The graphene content in the copper-based composite material is relatively low, resulting in a composite material with high strength, high elongation, and high electrical conductivity. The three-dimensional graphene network structure is beneficial for improving the reinforcement efficiency of the composite material.
[0061] This invention provides a three-dimensional graphene-reinforced copper-based composite material prepared by the preparation method described in the above technical solution.
[0062] The three-dimensional graphene-reinforced copper-based composite material prepared by this invention has higher tensile strength and electrical conductivity. Furthermore, due to the self-lubricating properties of graphene, it can effectively reduce adhesive wear and improve the wear resistance of the material.
[0063] The present invention also provides the application of the three-dimensional graphene-reinforced copper-based composite material described above in electronic and electrical equipment and power transmission switches.
[0064] The present invention does not impose any special limitations on the operation of the three-dimensional graphene-reinforced copper-based composite material in electronic and electrical equipment and power transmission switches. Any technical solution for the application of composite materials in electronic and electrical equipment and power transmission switches that is well known to those skilled in the art can be used.
[0065] The composite material prepared by this invention can be used as a contact switch material in the field of power transmission, which can effectively avoid power loss caused by deformation during long-term use of the switch; it can also be used as a substrate or lead frame in electronic equipment, which has high strength and high conductivity, as well as high thermal conductivity and high temperature stability.
[0066] The technical solutions of this invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0067] Example 1
[0068] (1) Place the copper foam substrate in a quartz boat and put it into a chemical vapor deposition tube furnace. Set the temperature control program to heat up to 900℃ in 90 minutes and then hold for 2 hours. During the heating and holding process, reducer gas H2 and protective gas Ar are introduced. The flow ratio of H2 to Ar is 20:300 and the total gas flow rate of H2 and Ar is 320 sccm. Annealing is performed to remove the oxide layer and impurities on the surface of the copper foam.
[0069] (2) Add PMMA particles to DMF solution, heat to 40°C, and stir magnetically until completely dissolved to prepare PMMA solution with a concentration of 1 mg / mL; place annealed copper foam in PMMA solution (PMMA solution should cover copper foam), heat to 50°C, ultrasonically impregnate for 15 min, then remove, place the PMMA-impregnated copper foam in drying oven, dry at 70°C for 12 h until the solvent is completely evaporated to obtain copper foam coated with PMMA.
[0070] (3) Place the foamed copper substrate coated with PMMA in a quartz boat, heat it to 900℃ and then keep it at that temperature for 1 hour. During the heating and holding process, reducer gas H2 and protective gas Ar are introduced. The flow ratio of H2 to Ar is 20:300 and the total gas flow rate of H2 and Ar is 320 sccm. Three-dimensional graphene structure is grown in situ.
[0071] (4) After the growth is completed, the carbon source in step (3) is exhausted, the temperature control system is turned off, the furnace body is manually opened, and the sample is rapidly cooled to room temperature. During the cooling process, reducing gas and protective gas are kept flowing in until the sample is cooled to room temperature. The graphene on the surface of the prepared foamed copper has good crystallinity and more than 10 layers, thus obtaining foamed copper loaded with graphene.
[0072] (5) The cooled copper-supported graphene foam samples were accumulated and placed in a graphite mold, then placed in a hot press furnace for hot pressing sintering. The sintering temperature was 900℃, the pressure was 40MPa, and the holding time was 1h. The heating rate was 10℃ / min, and the pressure program was set to 700℃-20MPa, 800℃-30MPa, and 900℃-40MPa. After the sintering program was completed, the samples were cooled with the furnace to obtain the three-dimensional graphene-reinforced copper-based composite material. The carbon content of the composite material was measured to be 0.08%, the tensile strength was 467MPa, the elongation was 20.5%, and the conductivity was 96.92% IACS.
[0073] Example 2
[0074] (1) Place the copper foam substrate in a quartz boat and put it into a chemical vapor deposition tube furnace. Set the temperature control program to heat up to 900℃ in 90 minutes and then hold for 2 hours. During the heating and holding process, reducer gas H2 and protective gas Ar are introduced. The flow ratio of H2 to Ar is 20:300 and the total gas flow rate of H2 and Ar is 320 sccm. Annealing is performed to remove the oxide layer and impurities on the surface of the copper foam.
[0075] (2) After annealing, the temperature was further increased to 1000℃ at a rate of 10℃ / min, and then held for 1 hour to grow three-dimensional graphene in situ. During graphene growth, a gaseous carbon source, CH4, was added at a flow rate of 20 sccm. After growth, the temperature control system was turned off, and the furnace body was manually opened to allow the sample to cool rapidly to room temperature. During cooling, the flow rates of the reducing gas and protective gas remained constant. The graphene on the surface of the prepared copper foam exhibited excellent crystallinity, with 1-3 layers, resulting in copper foam-supported graphene.
[0076] (3) The cooled copper-supported graphene foam samples were accumulated in a graphite mold and placed in a hot press furnace for hot pressing sintering. The sintering temperature was 900℃, the pressure was 40MPa, and the temperature and pressure were maintained for 1h. The heating rate was 10℃ / min, and the pressure program was set to 700℃-20MPa, 800℃-30MPa, and 900℃-40MPa. After the sintering program was completed, the samples were cooled with the furnace to obtain a high-strength and high-conductivity copper-based graphene composite material with three-dimensional graphene structure. The carbon content of the composite material was measured to be 0.06wt.%, the tensile strength was 458MPa, the elongation was 20%, and the conductivity was 97.05%IACS.
[0077] Example 3
[0078] (1) Place the copper foam substrate in a quartz boat and put it into a chemical vapor deposition tube furnace. Set the temperature control program to heat up to 900℃ in 90 minutes and then hold for 2 hours. During the heating and holding process, reducer gas H2 and protective gas Ar are introduced. The flow ratio of H2 to Ar is 20:300 and the total gas flow rate of H2 and Ar is 320 sccm. Annealing is performed to remove the oxide layer and impurities on the surface of the copper foam.
[0079] (2) After annealing, the gas flow rate remained constant, and the temperature was raised to 1000℃ at a rate of 10℃ / min, then held for 1 hour to grow three-dimensional graphene in situ. During graphene growth, a gaseous carbon source, CH4, was added at a flow rate of 2 sccm. After growth, the temperature control system was turned off, and the furnace body was manually opened to allow the sample to cool rapidly to room temperature. During cooling, the flow rates of the reducing gas and protective gas remained constant. The graphene on the surface of the prepared copper foam exhibited excellent crystallinity, with 3-5 layers, resulting in copper foam-supported graphene.
[0080] (3) The cooled copper-supported graphene foam samples were accumulated in a graphite mold and placed in a hot press furnace for hot pressing sintering. The sintering temperature was 900℃, the pressure was 40MPa, and the temperature and pressure were maintained for 1h. The heating rate was 10℃ / min, and the pressure program was set to 700℃-20MPa, 800℃-30MPa, and 900℃-40MPa. After the sintering program was completed, the samples were cooled with the furnace to obtain a high-strength and high-conductivity copper-based graphene composite material with three-dimensional graphene structure. The carbon content of the composite material was measured to be 0.07%, the tensile strength was 451MPa, the elongation was 21%, and the conductivity was 96.73% IACS.
[0081] The copper-supported graphene foam prepared in step (2) of Example 2 was observed using a scanning electron microscope (SEM). The SEM images obtained at different magnifications are shown below. Figure 1 As shown. (a) has a magnification of 500x, and (b) has a magnification of 5000x. From... Figure 1 As can be seen from (a) and (b), the surface of the copper foam is covered with graphene over a large area.
[0082] In summary, the three-dimensional graphene-reinforced copper-based composite material prepared by this invention has higher tensile strength and higher reinforcement efficiency.
[0083] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a three-dimensional graphene-reinforced copper-based composite material, comprising the following steps: (1) Place the foamed copper into a chemical vapor deposition tube furnace, introduce reducing gas and protective gas, raise the temperature, and anneal to remove the surface oxide layer and impurities to obtain pretreated foamed copper; the porosity of the foamed copper is 10~150 PPI; the reducing gas is H2, the protective gas is Ar, the flow ratio of reducing gas to protective gas is (1~100):300, and the total flow rate of reducing gas and protective gas is 1~1200 sccm; the annealing temperature is 500~1050℃, and the annealing time is 2~12h; (2) Add a carbon source to deposit and grow three-dimensional graphene on the pretreated foam copper surface obtained in step (1); the growth temperature of the three-dimensional graphene in step (2) is 800~1050℃ and the growth time is 1~5h; the carbon source includes gaseous carbon source, liquid carbon source or solid carbon source. (3) Deplete or turn off the carbon source in step (2), cool to room temperature, and obtain copper foam supported graphene; (4) The copper-supported graphene foam obtained in step (3) is densified to obtain a three-dimensional graphene-reinforced copper-based composite material; the densification method is hot pressing sintering, the densification temperature is 800~1000℃, the heating rate is 10~20℃ / min, the holding time is 0.5~2h, the pressure is 20~50MPa, and the cooling method is furnace cooling.
2. The three-dimensional graphene-reinforced copper-based composite material prepared by the preparation method of claim 1.
3. The application of the three-dimensional graphene-reinforced copper-based composite material according to claim 2 in electronic and electrical equipment and power transmission switches.
Citation Information
Patent Citations
Graphene-copper composite material preparation method
CN109811175A
Hot pressed sintering and chemical vapor deposition combined graphene copper composite material preparation method
CN114953620A
Graphene copper composite material preparation method based on combination of hot pressing sintering and chemical vapor deposition
WO2023216411A1