Method for electroplating heavy rare earth coating on surface of rare earth permanent magnet and application thereof
By using an electroplating method with an electrolyte molten salt system on the surface of rare earth permanent magnets, a heavy rare earth coating is formed at room temperature. This solves the problems of high-temperature side reactions and poor coating adhesion in existing technologies, and achieves low-cost, controllable thickness coating preparation, which is suitable for rare earth permanent magnets with complex shapes.
Patent Information
- Application Number
- CN202311565220.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-22
AI Technical Summary
Existing technologies for electroplating heavy rare earth coatings on the surface of rare earth permanent magnets suffer from problems such as high-temperature side reactions, high cost, low efficiency, poor adhesion, and uncontrollable coating thickness, making industrialization difficult.
Electroplating was performed at room temperature using an electrolyte molten salt system containing heavy rare earth elements. An electrolyte solution composed of heavy rare earth salts, metal salts, and additives was used to form a heavy rare earth coating on the surface of a rare earth permanent magnet through a three-electrode system. The electroplating conditions were controlled at -0.1 to -3V, and the electroplating time was 1 to 10 hours.
Stable heavy rare earth coating electroplating was achieved at room temperature, avoiding high-temperature side reactions, reducing costs, improving coating adhesion and thickness controllability, suitable for rare earth permanent magnets with complex shapes, and the electroplating solution can be reused.
Smart Images

Figure CN117604582B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of rare earth permanent magnet material surface treatment technology, and relates to a method for electroplating a heavy rare earth coating on the surface of a rare earth permanent magnet using an electrolyte molten salt system containing heavy rare earth salts that has good stability at room temperature, and its application. Background Technology
[0002] Neodymium iron boron (NdFeB) permanent magnets, due to their excellent magnetic properties, have crucial applications in high-end technology fields such as defense, information technology, communications, medical applications, automotive, and industrial motors. To improve the magnetic properties of magnets while reducing raw material costs, a heavy rare earth layer is typically deposited on the magnet surface, followed by grain boundary diffusion to achieve the desired magnetic properties. Common methods for depositing heavy rare earth layers include vapor deposition, sputtering, electrophoretic deposition, and coating. However, in practical applications, these methods suffer from various drawbacks, such as requirements on magnet shape, high energy consumption at high temperatures, uncontrollable coating thickness, poor adhesion, and poor stability of rare earth solutions. These factors result in high costs and low efficiency in mass industrial production. Rare earth coatings can be obtained in molten salt systems by adding fluorides and chlorides as electrolytes, but high temperatures often lead to various side reactions that affect coating formation, resulting in low preparation efficiency, high costs, and difficulty in industrialization.
[0003] Electroplating technology is mature in industrial production, with simple equipment and low cost. However, due to the strong chemical reactivity of rare earth elements, it is difficult to obtain an electroplated layer in aqueous solution due to the influence of hydrogen evolution. The published patent CN105839152A describes an electroplating process used to obtain a heavy rare earth layer in an organic system. The potential for this technology is 0.5–2V, and the electroplating duration is 20–500 minutes. First, electroplating is performed at a positive potential, which inevitably involves a vigorous hydrogen reduction reaction. Some hydrogen gas adsorbed on the magnet surface will weaken the adhesion of the heavy rare earth layer. Second, the NdFeB magnet acts as the cathode during electroplating. The positive potential causes corrosion and dissolution of the NdFeB magnet itself, leading to rapid changes in the solution composition and pH, prolonged electroplating time, and system instability. Furthermore, the NdFeB magnet's grain boundary neodymium-rich phase has a similar potential to the heavy rare earth elements. Electroplating-induced corrosion creates numerous pores on the magnet's surface. Prolonged electroplating time allows the solution to penetrate into the magnet, reducing its magnetic properties. In summary, the technical solution provided by patent CN105839152A results in waste of the magnet and rare earth elements in the solution, makes it difficult to control the stability of the electroplating process, and makes it difficult to obtain a high-quality coating. Summary of the Invention
[0004] The main objective of this invention is to provide a method for electroplating a heavy rare earth coating on the surface of a rare earth permanent magnet and its application, thereby overcoming the shortcomings of the prior art.
[0005] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:
[0006] This invention provides a method for electroplating a heavy rare earth coating on the surface of a rare earth permanent magnet, comprising:
[0007] Provides an electrolyte molten salt system containing heavy rare earth elements, comprising heavy rare earth salts and an electrolyte molten salt as a solvent;
[0008] Rare earth permanent magnets are placed in an electrolyte molten salt system containing heavy rare earth elements. The electrolyte molten salt system is used as the electrolyte, and the rare earth permanent magnets are used as the working electrodes. Electroplating is performed by passing an electric current through the system, thereby forming a heavy rare earth coating on the surface of the rare earth permanent magnets.
[0009] In some preferred embodiments, the heavy rare earth salt includes any one or a combination of two or more of the following: chlorides containing heavy rare earth elements, fluoroborates containing heavy rare earth elements, and trifluoromethanesulfonates containing heavy rare earth elements. In embodiments of the present invention, chlorides containing heavy rare earth elements and trifluoromethanesulfonates containing heavy rare earth elements are preferred as the heavy rare earth salts.
[0010] In some preferred embodiments, the electrolyte molten salt system containing heavy rare earth elements further includes metal salts and / or additives.
[0011] In some preferred embodiments, the electroplating is performed at a temperature of 20–80°C.
[0012] In some preferred embodiments, the electroplating lasts for 1 hour to 10 hours.
[0013] This invention also provides a heavy rare earth coating prepared by the method.
[0014] This invention also provides a rare earth permanent magnet with a surface coated with a heavy rare earth composite coating, prepared by the method.
[0015] Furthermore, embodiments of the present invention also provide the application of the aforementioned rare earth permanent magnet with a surface coated with a heavy rare earth composite coating in the diffusion of heavy rare earth grain boundaries.
[0016] Compared to existing technologies, the inventors of this invention have found that heavy rare earth element electroplating cannot be performed in aqueous solutions, and other electroplating systems have numerous limitations. For example, electroplating at high temperatures (above 800°C) can affect the NdFeB matrix, resulting in coarse grains and reduced magnetic properties. Furthermore, in existing solution-based electroplating systems, the NdFeB magnet's neodymium-rich phase has a similar potential to the reduced heavy rare earth elements, meaning most of the heavy rare earth elements adhere only to the main phase grains. Therefore, this invention creatively employs a molten salt electrolyte solution containing heavy rare earth elements as the electroplating system, applied to the preparation of heavy rare earth composite coatings on the surface of rare earth permanent magnets.
[0017] The beneficial effects of this invention also include at least the following:
[0018] 1) The method for electroplating heavy rare earth coatings on the surface of rare earth permanent magnets provided by this invention can reduce rare earth elements with large negative potentials at room temperature, enabling the electroplating of rare earth elements on sintered NdFeB magnets. The electroplating process has high chemical stability, can reduce rare earth elements with large negative potentials at room temperature, and does not corrode the substrate. It can also be applied to the surface of sintered NdFeB magnets with complex shapes. The electroplating solution system uses room temperature molten salt as electrolyte, which is stable, non-volatile, environmentally friendly, and reusable, avoiding the waste of rare earth resources caused by traditional coating methods.
[0019] 2) The room-temperature molten salt used in the method provided by this invention is composed of organic cations and inorganic or organic anions, which is insensitive to water and the environment, has high chemical stability, and does not directly react with NdFeB magnets. Meanwhile, the electroplating process used in this method is simple and low-cost, capable of preparing heavy rare earth coatings with controllable thickness and good adhesion on complex finished parts. After electroplating, the NdFeB magnets undergo heat treatment, resulting in varying degrees of increase in magnetic properties. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0021] Figure 1a and Figure 1b The images shown are scanning electron microscope (SEM) images and EDS spectra of the heavy rare earth coating prepared in Example 1 of this invention.
[0022] Figure 2a and Figure 2b The images shown are scanning electron microscope (SEM) images and EDS spectra of the heavy rare earth coating prepared in Example 4 of this invention.
[0023] Figure 3a and Figure 3b The images shown are scanning electron microscope (SEM) images and EDS spectra of the heavy rare earth coating prepared in Example 6 of this invention.
[0024] Figure 4a and Figure 4b The images shown are scanning electron microscope (SEM) images and EDS spectra of the heavy rare earth coating prepared in Comparative Example 1.
[0025] Figure 5a and Figure 5b The images are scanning electron microscope (SEM) images and EDS spectra of the heavy rare earth coatings prepared in Comparative Example 5, respectively.
[0026] Figure 6a and Figure 6b The images show the surface conditions of the magnets before and after electroplating in Comparative Example 7. Detailed Implementation
[0027] In view of the shortcomings of the prior art, the inventors of this invention, through long-term research and extensive practice, have proposed the technical solution of this invention. The technical problem to be solved by this invention is to provide the application of electroplating in the preparation of heavy rare earth coatings on the surface of rare earth permanent magnets, and a method for electroplating heavy rare earth coatings on the surface of rare earth permanent magnets. This method mainly employs an electrolyte molten salt system containing heavy rare earth salts with good stability at room temperature to electroplat the surface of NdFeB magnets to prepare heavy rare earth coatings. This invention specifically uses an electrolyte molten salt solution containing heavy rare earth elements as the electrolyte, applied in the preparation process of electroplating heavy rare earth composite coatings on the surface of rare earth permanent magnets. To further understand this invention, the following will further explain and illustrate the technical solution, its implementation process, and principles. However, it should be understood that these descriptions are only for further illustrating the features and advantages of this invention, and not for limiting the scope of the claims.
[0028] One aspect of this invention provides the application of electroplating in the preparation of heavy rare earth coatings on the surface of rare earth permanent magnets.
[0029] Furthermore, the electroplating method is an electroplating method using an electrolyte molten salt system containing heavy rare earth elements.
[0030] Furthermore, the electroplating method employs a counter electrode.
[0031] Another aspect of the present invention provides a method for electroplating a heavy rare earth coating on the surface of a rare earth permanent magnet, comprising:
[0032] Provides an electrolyte molten salt system containing heavy rare earth elements, comprising heavy rare earth salts and an electrolyte molten salt as a solvent;
[0033] Rare earth permanent magnets are placed in an electrolyte molten salt system containing heavy rare earth elements. The electrolyte molten salt system is used as the electrolyte, and the rare earth permanent magnets are used as the working electrodes. Electroplating is performed by passing an electric current through the system to form a heavy rare earth coating on the surface of the rare earth permanent magnets. The electroplating potential is -0.1 to -3V.
[0034] In some preferred embodiments of the present invention, the electroplating process can be carried out directly at room temperature without heating, and the electrolyte molten salt system containing heavy rare earth elements is in a liquid state at room temperature.
[0035] In this invention, the electrolyte molten salt is already in a liquid molten state at room temperature and does not require further melting. Temperature adjustment during the deposition process is solely for improving the conductivity of the electrolyte molten salt system, increasing the solubility of heavy rare earth salts in the system, and accelerating the electrochemical reaction rate. The electroplating solution system of this invention uses room-temperature molten salt as the electrolyte, which is reusable and avoids the resource waste and non-volatility of rare earth elements found in traditional processes; it can reduce rare earth elements with a large negative potential at room temperature.
[0036] In some preferred embodiments of the present invention, the electrolyte molten salt system containing heavy rare earth elements is used as an electroplating solution, which includes heavy rare earth salts and electrolyte molten salts as solvents.
[0037] In this invention, the electrolyte molten salt (i.e., solvent) is a commercially available room-temperature electrolyte molten salt, composed of organic cations and inorganic anions or organic anions. It is insensitive to water and the environment, has high chemical stability, and does not directly react with NdFeB magnets, thus effectively solving the problems existing in the prior art. The electrolyte molten salt preferably includes any one or more combinations of 1-ethyl-3-methylimidazolium tetrafluoroborate, trimethyl phosphate, and 1-butyl-1-methylpyrrolidine trifluoromethanesulfonate, more preferably 1-ethyl-3-methylimidazolium tetrafluoroborate, trimethyl phosphate, or 1-butyl-1-methylpyrrolidine trifluoromethanesulfonate, but is not limited thereto.
[0038] In some preferred embodiments of the present invention, the heavy rare earth salt includes any one or a combination of two or more of the following: chlorides containing heavy rare earth elements, fluoroborates containing heavy rare earth elements, and trifluoromethanesulfonates containing heavy rare earth elements, but is not limited thereto.
[0039] In some preferred embodiments of the present invention, the heavy rare earth elements contained in the electrolyte molten salt system containing heavy rare earth elements include Dy and / or Tb, more preferably Dy or Tb. Specifically, the heavy rare earth salt is selected from one of the following: chlorides of Dy or Tb (such as DyCl3, TbCl3), fluoroborates, trifluoromethanesulfonates (such as dysprosium trifluoromethanesulfonate (Dy(OTf)3), terbium trifluoromethanesulfonate (Tb(OTf)3)), but is not limited thereto.
[0040] In some preferred embodiments of the present invention, the concentration of heavy rare earth salts in the electrolyte molten salt system containing heavy rare earth elements is 0.1 to 10.0 mol / L, preferably 0.1 to 5 mol / L.
[0041] In some other preferred embodiments of the present invention, the electrolyte molten salt system containing heavy rare earth elements may further include metal salts and / or additives, preferably metal salts or additives.
[0042] Furthermore, if the electroplating uses an electrolyte molten salt system containing both heavy rare earth elements and metal elements, a heavy rare earth composite coating containing both heavy rare earth elements and metal elements is obtained.
[0043] In some embodiments, the metal salt contains any one or more of the following metal elements: Ti, Cr, Cu, Al, Pr, Nd, Ga, Zr, Nb, Hf, W, and V, but is not limited thereto.
[0044] Furthermore, the metal salt includes any one or a combination of two or more of the following: a chloride containing a metal element (e.g., CuCl2), a fluoroborate containing a metal element, and a trifluoromethanesulfonate containing a metal element (e.g., Cu(OTf)2), more preferably a chloride, a fluoroborate, or a trifluoromethanesulfonate, but not limited thereto.
[0045] In some preferred embodiments of the present invention, the concentration of the metal salt in the electrolyte molten salt system containing heavy rare earth elements is preferably 0.01 to 0.5 mol / L.
[0046] In some embodiments, the method includes: dissolving a metal salt in a solvent, and then adding a heavy rare earth salt to form an electrolyte molten salt system containing heavy rare earth elements and metal elements. Alternatively, in preparing the electrolyte molten salt system containing heavy rare earth salts, the metal salt is added first, and after it is completely dissolved in the solvent, the heavy rare earth salt is added.
[0047] In some embodiments, the additives include chemical reagents such as alcohols and / or esters that do not affect electroplating, with the aim of promoting the dissolution of heavy rare earth salts in room temperature molten salt. Preferably, they may include any one or a combination of two or more of anhydrous ethanol, ethylene glycol, and lithium chloride, more preferably anhydrous ethanol, ethylene glycol, or lithium chloride, but are not limited thereto. Specifically, the volume percentage of alcohols in the entire electrolyte solution (i.e., the electrolyte molten salt system) can be 10% to 50%. The role of the additives is to improve the solubility of heavy rare earth salts in the room temperature electrolyte molten salt system, increase the concentration of heavy rare earth ions, and improve the stability of the solution system. The additives may or may not be used.
[0048] In some preferred embodiments of the present invention, the concentration of the additive in the electrolyte molten salt system containing heavy rare earth elements is 0.01 to 0.5 mol / L.
[0049] Further, the method includes: dissolving heavy rare earth salts, metal salts and additives in a solvent by stirring to obtain the electrolyte molten salt system containing heavy rare earth elements, wherein the stirring time is 3 to 20 hours.
[0050] In some preferred embodiments of the present invention, the general formula of the rare earth permanent magnet is RE-MN-Fe-B, wherein RE includes any one or more combinations of praseodymium, neodymium, promethium, samarium, europium, gadolinium, holmium, erbium, thulium, ytterbium, lutetium, scandium, yttrium, etc., M includes any one or more combinations of terbium and dysprosium, and N includes any one or more combinations of lanthanum and cerium.
[0051] In some embodiments, the content of M in the RE-MN-Fe-B type rare earth permanent magnet is 0 to 0.5 wt%.
[0052] In some embodiments, the N content in RE-MN-Fe-B type rare earth permanent magnets is 0 to 10 wt%.
[0053] In some embodiments, the rare earth permanent magnet is a neodymium-based rare earth permanent magnet, which includes any one or more combinations of neodymium iron boron, neodymium-M iron boron, neodymium-N iron boron, and neodymium-MN iron boron, and is not limited thereto.
[0054] In some embodiments, the rare earth permanent magnet includes a rare earth permanent magnet blank that has been sintered, bonded, and hot-pressed.
[0055] In some embodiments, the rare earth permanent magnet includes a sintered rare earth permanent magnet obtained by sintering raw material powder through one or more steps such as melting, rapid solidification, crushing, hydrogen crushing, and orientation pressing.
[0056] Specifically, the matrix in this invention can be a neodymium-based rare earth permanent magnet (which can be neodymium iron boron, neodymium-cerium iron boron, neodymium-yttrium iron boron, etc.).
[0057] In some preferred embodiments, the present invention first pre-treats the magnet surface using a specific solution system composition: heavy rare earth salts, inorganic salts, organic salts, solvents, etc., with specific amounts and solution concentrations. Then, an electroplating process is carried out, combined with specific electroplating conditions, such as potential, deposition temperature, deposition time, etc., while controlling the coating preparation environment during the electroplating process, such as the range of water and oxygen content in the environment. Finally, the coating is post-treated and cleaned, thereby obtaining a coating with controllable thickness, especially capable of preparing thin coatings, and the coating has high density and adhesion, while the variation of heavy rare earth content in the coating is controllable.
[0058] In some preferred embodiments, the method further includes: first activating the rare earth permanent magnet, and then placing it in an electrolyte molten salt system containing heavy rare earth elements. In this invention, after the surface of the rare earth permanent magnet is activated, a heavy rare earth coating is electroplated onto its surface using an electroplating method.
[0059] Specifically, the method for electroplating a heavy rare earth composite coating on the surface of a rare earth permanent magnet includes the following steps: placing the sintered rare earth permanent magnet that has undergone activation treatment (also known as pretreatment) in an electrolyte molten salt solution containing heavy rare earth salts, and electroplating it by passing an electric current to obtain a sintered rare earth permanent magnet with a heavy rare earth coating on its surface.
[0060] Furthermore, the sintered rare earth permanent magnet preferably includes one or more steps of the raw material powder being smelted, cast, crushed, hydrogenated, and oriented pressing, and then sintered to obtain the sintered rare earth permanent magnet, more preferably multiple steps of smelting, casting, crushing, hydrogenated, and oriented pressing.
[0061] Furthermore, the activation treatment includes any one or a combination of two or more of the following steps: acid washing, organic solution cleaning, electrochemical activation, deionized water cleaning, and ultrasonic cleaning. More preferably, it includes acid washing, organic solution cleaning, electrochemical activation, deionized water cleaning, or ultrasonic cleaning, but is not limited thereto.
[0062] In some preferred embodiments of the present invention, the rare earth permanent magnet is directly electroplated with a heavy rare earth coating on its surface. The electroplating method employs a three-electrode system or a two-electrode system, more preferably a three-electrode system.
[0063] Furthermore, the rare-earth permanent magnet is preferably used as the working electrode.
[0064] In this invention, the counter electrode is preferably arranged parallel to the surface of the rare earth permanent magnet. Specifically, one counter electrode is parallel to one side of the rare earth permanent magnet to be coated with a heavy rare earth layer, and preferably arranged opposite to it.
[0065] In this invention, the electroplating method preferably uses an electrolyte molten salt system containing heavy rare earth elements and metal elements to obtain a heavy rare earth composite coating.
[0066] Furthermore, the energization includes direct current (DC) energization.
[0067] In some preferred embodiments of the present invention, the electroplating potential range is -0.1 to -3V.
[0068] In some preferred embodiments of the present invention, the electroplating temperature is 20–80°C.
[0069] In some preferred embodiments of the present invention, the electroplating process lasts for 1 hour to 10 hours.
[0070] More specifically, the electroplating process uses a three-electrode system, with a sintered NdFeB magnet as the cathode and a platinum sheet as the anode. A DC constant potential is applied, with a potential range of -0.1 to -3V, a deposition temperature of 20 to 80°C, and a deposition time of 1 to 10 hours.
[0071] In some preferred embodiments of the present invention, the oxygen content of the electrolyte molten salt system during the electroplating process is controlled between 10 and 300 ppm. Specifically, it is better to have no oxygen during the electroplating process of the present invention, but the presence of a small amount of oxygen does not have a significant impact on the experiment.
[0072] In some preferred embodiments of the present invention, the water content of the electrolyte molten salt system during the electroplating process is controlled at 10 to 200 ppm.
[0073] This invention aims to complete and refine the overall technical solution, better improve the electroplating effect, and further enhance the uniformity and density of the heavy rare earth coating on the surface of rare earth permanent magnets. Specifically, the method for electroplating a heavy rare earth coating on the surface of rare earth permanent magnets may include the following:
[0074] The purpose of the pretreatment of the sintered NdFeB magnet surface is to remove the oxide layer on the sintered NdFeB surface and expose the substrate surface.
[0075] The preparation of room temperature molten salt electrolyte involves dissolving heavy rare earth salts, metal salts, and additives into room temperature molten salt through stirring or heating, thus obtaining a room temperature electrolyte molten salt system.
[0076] The electroplating process yields sintered NdFeB magnets with a coating containing heavy rare earth elements.
[0077] In the post-processing stage, the electroplated magnet is cleaned to obtain a heavy rare earth coating.
[0078] Furthermore, the stirring can be magnetic stirring, and the magnetic stirring lasts for 3 to 20 hours.
[0079] Furthermore, the method also includes post-treatment of the obtained heavy rare earth coating. Specifically, the post-treatment includes sequentially cleaning with water and anhydrous ethanol, followed by drying, or cleaning with an organic solvent.
[0080] Furthermore, the post-treatment involves rinsing with deionized water and anhydrous ethanol in sequence and then drying, or rinsing with other organic solvents such as acetonitrile, dimethyl carbonate, etc.
[0081] In summary, the method and equipment of this invention are simple and low-cost. In the solution system provided in this invention, heavy rare earth elements can be effectively electroplated onto the surface of the treated NdFeB magnet. Furthermore, this method is environmentally friendly and can produce heavy rare earth coatings with controllable thickness and content on complex shaped parts. The solution system is stable during the preparation process, with no additional products generated, thus solving the key technical problem of electroplating heavy rare earth coatings on the surface of rare earth permanent magnets. The method of this invention can electroplat rare earth elements on the surface of sintered NdFeB magnets, the electroplating process is stable, there is no corrosion to the substrate, and it can be applied to the surface of sintered NdFeB magnets with complex shapes.
[0082] Another aspect of the present invention provides a heavy rare earth coating prepared by the aforementioned method.
[0083] In some preferred embodiments of the present invention, the thickness of the heavy rare earth coating is 100 nm to 50 μm.
[0084] In some preferred embodiments of the present invention, the content of rare earth elements in the heavy rare earth coating is 15-45 wt%.
[0085] In this invention, the heavy rare earth composite coating preferably includes heavy rare earth elements, or heavy rare earth elements and metallic elements. The types of heavy rare earth elements and metallic elements are described above.
[0086] Another aspect of the present invention provides a rare earth permanent magnet with a heavy rare earth composite coating on its surface, prepared by the aforementioned method.
[0087] In this invention, the heavy rare earth composite coating prepared by surface electroplating is a raw material for heavy rare earth grain boundary diffusion in rare earth permanent magnets. Specifically, the sintered rare earth permanent magnet with the heavy rare earth composite coating on its surface is preferably a raw material for heavy rare earth grain boundary diffusion in sintered rare earth permanent magnets.
[0088] This invention also provides the application of sintered rare earth permanent magnets with heavy rare earth coatings on their surfaces prepared by the preparation method described in any of the above technical solutions in the diffusion of heavy rare earth grain boundaries in sintered rare earth permanent magnets.
[0089] In this invention, the specific application is that the sintered rare earth permanent magnet with a heavy rare earth coating on its surface prepared by this invention is used as a raw material for heavy rare earth grain boundary diffusion in sintered rare earth permanent magnets. That is, after diffusion treatment, the sintered rare earth permanent magnet with a heavy rare earth coating on its surface yields a rare earth permanent magnet product with grain boundary diffusion.
[0090] In summary, this invention enables the electroplating of rare earth elements onto the surface of rare earth permanent magnets. The electroplating solution system is uniform, reusable, and the electroplating process is stable, non-volatile, and does not corrode the substrate. Rare earth elements with large negative potentials can be reduced at room temperature, avoiding the resource waste associated with traditional coating methods. The process equipment is simple and low-cost. Traditional aqueous and acidic plating solutions cannot achieve the electroplating of heavy rare earth elements. This method enables the electroplating of heavy rare earth coatings onto activated magnet surfaces, and can produce thick, well-bonded heavy rare earth coatings on complex-shaped magnets, with no limitations on substrate shape or specifications. After electroplating, the magnets undergo heat treatment, resulting in varying degrees of increase in magnetic properties.
[0091] To further illustrate the present invention, the following describes in detail, with reference to embodiments, the application of the electroplating method provided by the present invention in electroplating heavy rare earth composite coatings on the surface of rare earth permanent magnets, and a method for electroplating heavy rare earth composite coatings on the surface of rare earth permanent magnets. However, it should be understood that these embodiments are implemented under the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operating procedures, only to further illustrate the features and advantages of the present invention, and not to limit the scope of protection of the claims of the present invention. The scope of protection of the present invention is not limited to the following embodiments.
[0092] There are no particular restrictions on the source of any raw materials used in this invention; they can be purchased from the market or prepared using conventional methods known to those skilled in the art.
[0093] There are no particular restrictions on the purity of any of the raw materials used in this invention. However, this invention preferably uses industrial-grade pure materials or materials with conventional purity used in the preparation of electroplated coatings on the surface of NdFeB magnets.
[0094] All raw materials of this invention are conventional in the field, and each brand name and abbreviation is clear and distinct in its relevant application. Those skilled in the art can purchase them from the market or prepare them by conventional methods based on the brand name, abbreviation and corresponding application.
[0095] All processes and equipment in this invention are conventional names in the field, and each name is clear and unambiguous in its relevant application. Those skilled in the art can understand the conventional process steps and corresponding equipment used based on the name.
[0096] Example 1
[0097] Commercial magnets of grade N48 (Dy0Ce5wt%) with a specification of Φ10*4mm were subjected to acid cleaning and activation treatment in a dilute nitric acid solution with a volume ratio of 1:24 (nitric acid:deionized water) using an ultrasonic cleaner. After rinsing with deionized water, they were dried and ready for use. In a glove box (with high-purity argon gas protection throughout the operation, and oxygen content controlled below 300ppm and water content below 200ppm), 50mL of... 1-Ethyl-3-methylimidazolium tetrafluoroborate was used as the solvent (EMIMBF4). 0.1 mol / L DyCl3 was added to the solvent in batches (anhydrous ethanol, ethylene glycol, and lithium chloride could be added during this process to improve the solubility of the system; the concentration of the additive was 0.1 mol / L). The addition process was carried out using a magnetic stirrer for 3 hours until DyCl3 was completely dissolved. During the electroplating process, a platinum sheet was used as the counter electrode, a neodymium iron boron magnet as the working electrode, and Ag / AgCl as the reference electrode. The constant potential was provided by an electrochemical workstation. The electroplating process was set to a potential of -0.1 V, a temperature of room temperature (approximately 20°C), and a plating duration of 1 hour. After electroplating, the plating surface was rinsed with dimethyl carbonate and finally dried with cold air.
[0098] The inventors in this case performed scanning electron microscopy and EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth coatings. The results are shown in [reference needed]. Figure 1a and Figure 1b The adhesion of the coating was tested using a scratch tester. The results of the Dy content and adhesion in the coating are shown in Table 1.
[0099] Example 2
[0100] The difference between this embodiment and Example 1 is as follows: First, 0.01 mol / L CuCl2 is added to 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIMBF4) as a solvent. After the CuCl2 is completely dissolved, 0.5 mol / L LyCl3 is added in batches to the mixed solvent of EMIMBF4 and CuCl2 (any one of anhydrous ethanol, ethylene glycol, and lithium chloride can be added during this process to improve the solubility of the system). The mixture is stirred continuously with a magnetic stirrer for 5 hours. The electroplating potential is set to -0.5V, and the temperature of the electroplating tank is adjusted to 40°C (maintaining a constant temperature from solution preparation to the entire electroplating process). The electroplating duration is 2 hours, and other conditions remain unchanged.
[0101] The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating and tested the coating adhesion using a scratch tester. The Dy content and adhesion results in the coating are shown in Table 1.
[0102] Example 3
[0103] The difference between this embodiment and Embodiment 2 is as follows: A commercial magnet of grade N48 with a specification of 10*4mm was acid-washed using an ultrasonic cleaner in a dilute nitric acid solution with a volume ratio of 1:24 (nitric acid:deionized water). The magnet was then surface-activated in an acetone solution, followed by rinsing with deionized water and drying. First, 0.05 mol / L CuCl2 was added to trimethyl phosphate as a solvent. After the CuCl2 was completely dissolved, 1 mol / L LyCl3 was added in batches to the mixed solvent of trimethyl phosphate and CuCl2. The mixture was continuously stirred with a magnetic stirrer for 8 hours. The electroplating process was set to a potential of -1.5V, and the electroplating tank temperature was adjusted to 60℃ (maintaining a constant temperature from solution preparation to the entire electroplating process). The electroplating duration was 5 hours, with other conditions remaining unchanged.
[0104] The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating and tested the coating adhesion using a scratch tester. The Dy content and adhesion results in the coating are shown in Table 1.
[0105] Example 4
[0106] The difference between this embodiment and Example 3 is that the commercial magnet of grade N48 (Dy0Ce5wt%) is replaced with a commercial magnet of N48 (Dy0Ce0) with a specification of 10*4mm, while the pretreatment conditions remain unchanged. First, 0.01mol / L CuCl2 is added to 1-ethyl-3-methylimidazolium tetrafluoroborate as a solvent. After the CuCl2 is completely dissolved, 0.5mol / L dysprosium trifluoromethanesulfonate (Dy(OTf)3) is added in batches to a mixed solvent of EMIMBF4 and CuCl2 (any one of anhydrous ethanol, ethylene glycol, and lithium chloride can be added during this process to improve the solubility of the system). The mixture is stirred continuously with a magnetic stirrer for 8 hours. The electroplating potential is set to -1.7V, and the electroplating tank temperature is adjusted to 20℃ (maintaining a constant temperature from solution preparation to the entire electroplating process). The electroplating duration is 5 hours, and other conditions remain unchanged.
[0107] The inventors in this case performed scanning electron microscopy and EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating. The results are shown in [reference needed]. Figure 2a and Figure 2b The adhesion of the coating was tested using a scratch tester. The results of the Dy content and adhesion in the coating are shown in Table 1.
[0108] Example 5
[0109] The difference between this embodiment and Example 4 is that the metal salt CuCl2 is replaced with AlCl3 and added to 1-ethyl-3-methylimidazolium tetrafluoroborate as a solvent, the electroplating process is set to a potential of -1.8V, and other conditions remain unchanged.
[0110] The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating and tested the coating adhesion using a scratch tester. The Dy content and adhesion results in the coating are shown in Table 1.
[0111] Example 6
[0112] The difference between this embodiment and Example 4 is as follows: First, 0.1 mol / L Cu(OTf)2 is added to 1-butyl-1-methylpyrrolidine trifluoromethanesulfonate as a solvent. After Cu(OTf)2 is completely dissolved, 2 mol / L dysprosium trifluoromethanesulfonate (Dy(OTf)3) is added in batches to the mixed solvent of 1-butyl-1-methylpyrrolidine trifluoromethanesulfonate and Cu(OTf)2 (any one of anhydrous ethanol, ethylene glycol, and lithium chloride can be added during this process to improve the solubility of the system). The mixture is stirred continuously with a magnetic stirrer for 10 hours. The electroplating process is set to a potential of -1.5V, and the electroplating tank temperature is adjusted to 20°C (maintaining a constant temperature from solution preparation to the entire electroplating process). The electroplating duration is 8 hours, and other conditions remain unchanged.
[0113] The inventors in this case performed scanning electron microscopy and EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating. The results are shown in [reference needed]. Figure 3a and Figure 3b The adhesion of the coating was tested using a scratch tester. The results of the Dy content and adhesion in the coating are shown in Table 1.
[0114] Example 7
[0115] The difference between this embodiment and Example 6 is that 2 mol / L terbium trifluoromethanesulfonate Tb(OTf)3 was measured and added in batches to a mixed solvent of 1-butyl-1-methylpyrrolidine trifluoromethanesulfonate and Cu(OTf)2, while other conditions remained unchanged.
[0116] The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating and tested the coating adhesion using a scratch tester. The Tb content and adhesion results in the coating are shown in Table 1.
[0117] Example 8
[0118] The difference between this embodiment and Example 6 is that a commercial magnet of grade N48 (Dy0Ce0) with a specification of 10*4mm was electrochemically activated, rinsed with deionized water, and dried for later use. First, 0.1 mol / L CuCl2 was added to 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIMBF4) as a solvent. After the CuCl2 was completely dissolved, 1 mol / L DyCl3 was added in batches to the mixed solvent of EMIMBF4 and CuCl2 (any one of anhydrous ethanol, ethylene glycol, and lithium chloride could be added during this process to improve the solubility of the system). The mixture was continuously stirred with a magnetic stirrer for 10 hours. The electroplating potential was set to -1.8V, and the electroplating tank temperature was adjusted to 40℃ (maintaining a constant temperature from solution preparation to the entire electroplating process). The electroplating duration was 8 hours, with other conditions remaining unchanged.
[0119] The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating and tested the coating adhesion using a scratch tester. The Dy content and adhesion results in the coating are shown in Table 1.
[0120] Example 9
[0121] The difference between this embodiment and embodiment 6 is that the metal salt CuCl2 is changed to AlCl3, while other conditions remain the same.
[0122] The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating and tested the coating adhesion using a scratch tester. The Dy content and adhesion results in the coating are shown in Table 1.
[0123] Example 10
[0124] The difference between this embodiment and Example 8 is that the commercial magnet of grade N48 (Dy0Ce0) is replaced with a commercial magnet of grade N50 (Dy0.5wt%Ce0) with a specification of 10*4mm. Electrochemical activation treatment is performed, followed by rinsing with deionized water and drying. First, 0.2 mol / L CuCl2 is added to 1-ethyl-3-methylimidazolium tetrafluoroborate (EMIMBF4) as a solvent. After the CuCl2 is completely dissolved, 1 mol / L DyCl3 is added in batches to the mixed solvent of EMIMBF4 and CuCl2. The mixture is continuously stirred with a magnetic stirrer for 15 hours. The electroplating potential is set to -2V, and the electroplating tank temperature is adjusted to 60℃ (maintaining a constant temperature from solution preparation to the entire electroplating process). The electroplating duration is 8 hours, with other conditions remaining unchanged.
[0125] The inventors of this case conducted scanning electron microscopy and EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating, and tested the coating adhesion by scratch tester. The Dy content and adhesion results in the coating are shown in Table 1.
[0126] Example 11
[0127] The difference between this embodiment and Example 10 is that the metal salt CuCl2 is changed to Al(OTf)3, the heavy rare earth salt DyCl3 is changed to TbCl3, and other conditions remain the same.
[0128] The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating and tested the coating adhesion using a scratch tester. The Tb content and adhesion results in the coating are shown in Table 1.
[0129] Example 12
[0130] The difference between this embodiment and Example 10 is that Cu(OTf)2 was added to 1-butyl-1-methylpyrrolidine trifluoromethanesulfonate as a solvent. After Cu(OTf)2 was completely dissolved, 1 mol / L dysprosium trifluoromethanesulfonate (Dy(OTf)3) was measured and added in batches to the mixed solvent of 1-butyl-1-methylpyrrolidine trifluoromethanesulfonate and Cu(OTf)2. The mixture was continuously stirred with a magnetic stirrer for 15 hours. The electroplating process potential was set to -1.5V, and the electroplating tank temperature was adjusted to 20°C (maintaining a constant temperature from solution preparation to the entire electroplating process). The electroplating duration was 10 hours, with other conditions remaining unchanged.
[0131] The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating and tested the coating adhesion using a scratch tester. The Dy content and adhesion results in the coating are shown in Table 1.
[0132] Example 13
[0133] The difference between this embodiment and embodiment 12 is that Cu(OTf)2 is changed to Al(OTf)3, the electroplating process potential is set to -1.9V, and other conditions remain unchanged.
[0134] The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating and tested the coating adhesion using a scratch tester. The Dy content and adhesion results in the coating are shown in Table 1.
[0135] Example 14
[0136] The difference between this embodiment and Example 8 is that the commercial magnet of grade N50 (Dy 0.5wt% Ce 0) was replaced with a commercial magnet of N50 (Dy 0.5wt% Ce 10wt%), which underwent electrochemical activation treatment, and was then rinsed with deionized water and dried for later use. First, 0.3 mol / L Cu(OTf)2 was added to 1-butyl-1-methylpyrrolidine trifluoromethanesulfonate as a solvent. After the Cu(OTf)2 was completely dissolved, 3 mol / L dysprosium trifluoromethanesulfonate (Dy(OTf)3) was added in batches to the mixed solvent of 1-butyl-1-methylpyrrolidine trifluoromethanesulfonate and Cu(OTf)2. The mixture was continuously stirred with a magnetic stirrer for 20 hours. The electroplating potential was set to -1.8V, the electroplating tank temperature was adjusted to 40℃ (maintaining a constant temperature from solution preparation to the entire electroplating process), and the electroplating duration was 10 hours, with other conditions remaining unchanged.
[0137] The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating and tested the coating adhesion using a scratch tester. The Dy content and adhesion results in the coating are shown in Table 1.
[0138] Example 15
[0139] The difference between this embodiment and Example 9 is as follows: First, 0.5 mol / L Cu(OTf)₂ is added to trimethyl phosphate as a solvent. After the Cu(OTf)₂ is completely dissolved, 5 mol / L dysprosium trifluoromethanesulfonate Dy(OTf)₃ is added in batches to the mixed solvent of trimethyl phosphate and Cu(OTf)₂. The mixture is continuously stirred with a magnetic stirrer for 20 hours. The electroplating potential is set to -3V, and the electroplating tank temperature is adjusted to 80℃ (maintaining a constant temperature from solution preparation to the entire electroplating process). The electroplating duration is 10 hours, with other conditions remaining unchanged.
[0140] The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the prepared heavy rare earth composite coating and tested the coating adhesion using a scratch tester. The Dy content and adhesion results in the coating are shown in Table 1.
[0141] Comparative Example 1
[0142] Commercial magnets of grade N48 (Dy0Ce 5wt%) with a specification of 10*4mm were acid-washed and activated using an ultrasonic cleaner in a dilute nitric acid solution with a volume ratio of 1:24 (nitric acid:deionized water). After rinsing with deionized water, they were dried for later use. First, 1 mol / L Fe(BF4)2 was added to the solvent 1-ethyl-3-methylimidazolium tetrafluoroborate. Then, 1 mol / L LyCl3 was added to the mixed solvent of Fe(BF4)2 and 1-ethyl-3-methylimidazolium tetrafluoroborate. The addition process was continuously stirred with a magnetic stirrer for 15 hours. During the electroplating process, a platinum sheet was used as the counter electrode, a neodymium iron boron magnet as the working electrode, and Ag / AgCl as the reference electrode. The constant potential was provided by an electrochemical workstation. The electroplating process was set to a potential of -1.5V, and the electroplating tank temperature was adjusted to 40℃ (maintained at a constant temperature from solution preparation to the entire electroplating process). The electroplating duration was 8 hours.
[0143] The inventors in this case performed scanning electron microscopy and EDS energy dispersive spectroscopy analysis on the surface of the electroplated magnet. The results are shown in [link to relevant documentation]. Figure 4a and Figure 4b As can be seen, the grains on the surface of the magnet were corroded, with obvious pores and corrosion zones appearing. There were also a small number of aggregated Dy particles on the surface. The results are shown in Table 1.
[0144] Comparative Example 2
[0145] The difference between this comparative example and Comparative Example 1 is that: first, 0.5 mol / L Co(BF4)2 was added to the solvent 1-ethyl-3-methylimidazolium tetrafluoroborate, and then 1 mol / L DyCl3 was added to the mixed solvent of Co(BF4)2 and 1-ethyl-3-methylimidazolium tetrafluoroborate, while other conditions remained unchanged.
[0146] During the solution preparation process, when DyCl3 is added, DyCl3 is basically insoluble in the mixed solvent of Co(BF4)2 and 1-ethyl-3-methylimidazolium tetrafluoroborate, and a uniform electroplating solution cannot be obtained. No obvious reduction reaction occurs during the electroplating process. The inventors of this case performed EDS energy dispersive spectroscopy analysis on the surface of the electroplated magnet, and the results are shown in Table 1. There is no reduction of Dy and Cu elements on the surface of the magnet.
[0147] Comparative Example 3
[0148] The difference between this comparative example and Comparative Example 1 is that a commercial magnet of grade N50 (Dy 0.5wt% Ce0) with a specification of 10*4mm was acid-washed, rinsed with deionized water, and then dried for later use. First, 1 mol / L Fe(BF4)2 was added to the solvent 1-ethyl-3-methylimidazolium tetrafluoroborate. Then, 1 mol / L Dy(OTf)3 was added to the mixed solvent of Fe(BF4)2 and 1-ethyl-3-methylimidazolium tetrafluoroborate. The electroplating process was set to a potential of 1V, with other conditions remaining unchanged.
[0149] During the electroplating process, a large number of bubbles are generated in the solution, resulting in severe corrosion on the magnet surface and the shedding of magnet particles. The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the surface of the electroplated magnet, and the results are shown in Table 1. No Dy or Cu elements were reduced on the magnet surface.
[0150] Comparative Example 4
[0151] The difference between this comparative example and comparative example 3 is that: first, 0.5 mol / L Co(BF4)2 was added to the solvent 1-ethyl-3-methylimidazolium tetrafluoroborate, and then 1 mol / L Dy(OTf)3 was added to the mixed solvent of Co(BF4)2 and 1-ethyl-3-methylimidazolium tetrafluoroborate, while other conditions remained unchanged.
[0152] During the electroplating process, a large number of bubbles are generated in the solution, resulting in severe corrosion on the magnet surface and the shedding of magnet particles. The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the surface of the electroplated magnet, and the results are shown in Table 1. No Dy or Cu elements were reduced on the magnet surface.
[0153] Comparative Example 5
[0154] The difference between this comparative example and Comparative Example 1 is that the commercial magnet of grade N48 (Dy0Ce5wt%) was replaced with a commercial magnet of N48 (Dy0Ce0) with a specification of 10*4mm. After acid washing and activation treatment, it was rinsed with deionized water and dried for later use. First, 1 mol / L Fe(BF4)2 and 0.5 mol / L Co(BF4)2 were measured and mixed evenly, and then added to the solvent 1-ethyl-3-methylimidazolium tetrafluoroborate. Then, 1 mol / L LyCl3 was measured and added to the mixed solvent of Fe(BF4)2, Co(BF4)2 and 1-ethyl-3-methylimidazolium tetrafluoroborate. The electroplating process was set to a potential of 1V, and other conditions remained unchanged.
[0155] During solution preparation, when DyCl3 is added, the solution becomes turbid and separates into layers. DyCl3 is basically insoluble in the mixed solvent of Fe(BF4)2, Co(BF4)2 and 1-ethyl-3-methylimidazolium tetrafluoroborate. During the electroplating process, a large number of bubbles are generated in the solution.
[0156] The inventors in this case performed scanning electron microscopy and EDS energy dispersive spectroscopy analysis on the surface of the electroplated magnet. The results are shown in [link to relevant documentation]. Figure 5a and Figure 5b As can be seen, the magnet surface is severely corroded, accompanied by the shedding of magnet particles, and there is no reduction of Dy and Cu elements on the magnet surface.
[0157] Comparative Example 6
[0158] The difference between this comparative example and Comparative Example 5 is that a commercial magnet of grade N50 (Dy 0.5wt% Ce10) with a specification of 10*4mm was used. After acid washing, it was rinsed with deionized water and dried for later use. First, 1 mol / L Fe(BF4)2 and 0.5 mol / L Co(BF4)2 were measured and mixed evenly, and then added to the solvent 1-ethyl-3-methylimidazolium tetrafluoroborate. Then, 1 mol / L Dy(OTf)3 was measured and added to the mixed solvent of Fe(BF4)2, Co(BF4)2 and 1-ethyl-3-methylimidazolium tetrafluoroborate. Other conditions remained unchanged.
[0159] During the electroplating process, a large number of bubbles are generated in the solution, resulting in severe corrosion on the magnet surface and the shedding of magnet particles. The inventors of this case conducted EDS energy dispersive spectroscopy analysis on the surface of the electroplated magnet, and the results are shown in Table 1. No Dy or Cu elements were reduced on the magnet surface.
[0160] Comparative Example 7
[0161] The difference between this comparative example and Example 4 is that 1-ethyl-3-methylimidazolium tetrafluoroborate was replaced with an aqueous solution as the solvent, while other conditions remained unchanged. During the electroplating process, a large number of bubbles were generated in the solution, severe corrosion occurred on the magnet surface, accompanied by the shedding of magnet particles, and no reduction of Dy or Cu elements was observed.
[0162] In this comparative example, the states of the magnet surface before and after electroplating are respectively shown in [reference 1]. Figure 6a and Figure 6b .
[0163] Comparative Example 8
[0164] The difference between this comparative example and Example 6 is that the electroplating process was set to a potential of 1V, while other conditions remained unchanged. The electroplating process exhibited a violent reaction, the solution system rapidly turned reddish-brown, a large number of bubbles were generated, large magnetic particles detached, and there was no reduction of Dy or Cu elements.
[0165] Table 1. Test results of Dy and Cu content and coating adhesion in the coatings prepared in each example and comparative example.
[0166]
[0167]
[0168] In addition, the inventors of this case also conducted experiments with other raw materials, process operations, and process conditions described in this specification, referring to the aforementioned embodiments, and obtained relatively ideal results in all cases.
[0169] The method for electroplating a heavy rare earth coating on the surface of a rare earth permanent magnet, provided by this invention, has been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this invention. The descriptions of the embodiments above are merely to help understand the method and core ideas of this invention, including the best mode, and to enable any person skilled in the art to practice this invention, including manufacturing and using any device or system, and implementing any combined method. It should be noted that for those skilled in the art, several improvements and modifications can be made to this invention without departing from the principles of this invention, and these improvements and modifications also fall within the protection scope of the claims of this invention. The scope of protection of this patent is defined by the claims and may include other embodiments that can be conceived by those skilled in the art. If these other embodiments have structural elements that are not different from the wording of the claims, or if they include equivalent structural elements that are not substantially different from the wording of the claims, then these other embodiments should also be included within the scope of the claims.
Claims
1. A method for electroplating a heavy rare earth coating on the surface of a rare earth permanent magnet, characterized in that, include: A molten electrolyte salt system containing heavy rare earth elements is provided. The molten electrolyte salt system is liquid at room temperature and comprises a heavy rare earth salt and a molten electrolyte salt as a solvent. The heavy rare earth salt is selected from any one or a combination of two or more of heavy rare earth element-containing chlorides, heavy rare earth element-containing fluoroborates, and heavy rare earth element-containing trifluoromethanesulfonates. The heavy rare earth element contained in the molten electrolyte salt system is selected from Dy and / or Tb. The molten electrolyte salt is composed of an organic cation and an inorganic anion or an organic anion, selected from 1-ethyl-3- The electrolyte molten salt system containing heavy rare earth elements comprises any one or a combination of two or more of methylimidazolium tetrafluoroborate, trimethyl phosphate, and 1-butyl-1-methylpyrrolidine trifluoromethanesulfonate; the electrolyte molten salt system further comprises a metal salt and an additive, wherein the metal salt contains a metal element selected from Cu and Al, and the additive is selected from any one or a combination of two or more of anhydrous ethanol, ethylene glycol, and lithium chloride; the concentration of the heavy rare earth salt in the electrolyte molten salt system containing heavy rare earth elements is 0.1~10.0 mol / L, and the concentration of the metal salt is 0.01~0.5 mol / L. Rare earth permanent magnets are placed in an electrolyte molten salt system containing heavy rare earth elements. A three-electrode system is used, with the electrolyte molten salt system as the electrolyte and the rare earth permanent magnet as the working electrode. The counter electrode is set parallel to the surface of the rare earth permanent magnet. Electroplating is performed by applying current, thereby forming a heavy rare earth coating containing heavy rare earth elements and metallic elements on the surface of the rare earth permanent magnet. The current application includes direct current, the electroplating potential is -0.1 ~ -3V, the electroplating temperature is 20 ~ 80℃, the electroplating duration is 1h ~ 10h, the oxygen content of the electrolyte molten salt system during the electroplating process is 10 ~ 300ppm, and the water content of the electrolyte molten salt system during the electroplating process is 10 ~ 200ppm.
2. The method according to claim 1, characterized in that: The concentration of heavy rare earth salts in the electrolyte molten salt system containing heavy rare earth elements is 0.1~5 mol / L.
3. The method according to claim 1, characterized in that: The metal salt is selected from any one or a combination of two or more of the following: chlorides containing metal elements, fluoroborates containing metal elements, and trifluoromethanesulfonates containing metal elements.
4. The method according to claim 1, characterized in that... include: Metal salts are dissolved in a solvent, and then heavy rare earth salts are added to form an electrolyte molten salt system containing heavy rare earth elements and metal elements.
5. The method according to claim 1, characterized in that: The concentration of additives in the electrolyte molten salt system containing heavy rare earth elements is 0.01~0.5 mol / L.
6. The method according to claim 1, characterized in that... include: The heavy rare earth salt, metal salt and additives are dissolved in a solvent by stirring to obtain the electrolyte molten salt system containing heavy rare earth elements. The stirring time is 3 to 20 hours.
7. The method according to claim 1, characterized in that: The general formula of the rare earth permanent magnet is RE-MN-Fe-B, wherein RE is selected from any one or more combinations of praseodymium, neodymium, promethium, samarium, europium, gadolinium, holmium, erbium, thulium, ytterbium, lutetium, scandium, and yttrium; M is selected from any one or two combinations of terbium and dysprosium; and N is selected from any one or two combinations of lanthanum and cerium.
8. The method according to claim 7, characterized in that: The content of M in the rare earth permanent magnet is 0~0.5wt%.
9. The method according to claim 7, characterized in that: The N content in the rare earth permanent magnet is 0~10wt%.
10. The method according to claim 7, characterized in that: The rare earth permanent magnet is a neodymium-based rare earth permanent magnet; the neodymium-based rare earth permanent magnet is selected from any one or a combination of two or more of neodymium iron boron, neodymium-M iron boron, neodymium-N iron boron and neodymium-MN iron boron.
11. The method according to claim 7, characterized in that: The rare earth permanent magnet is a rare earth permanent magnet blank that has been sintered, bonded and hot-pressed.
12. The method according to claim 7, characterized in that: The rare earth permanent magnet includes a sintered rare earth permanent magnet obtained by sintering raw material powder through one or more steps such as melting, rapid solidification, crushing, hydrogen crushing, orientation pressing and molding.
13. The method according to claim 1, characterized in that, Also includes: The rare earth permanent magnet is first activated and then placed in an electrolyte molten salt system containing heavy rare earth elements; wherein the activation treatment is any one or a combination of two or more of the following: acid washing, organic solution cleaning, electrochemical activation, deionized water cleaning and ultrasonic cleaning.
14. The method according to claim 1, characterized in that, Also includes: The obtained heavy rare earth coating is subjected to post-treatment, which involves first cleaning with water and then anhydrous ethanol, followed by drying, or cleaning with an organic solvent.
15. The method according to claim 14, characterized in that: The organic solvent is selected from acetonitrile and / or dimethyl carbonate.
16. A heavy rare earth coating prepared by any one of claims 1-15, wherein the content of rare earth elements in the heavy rare earth coating is 15-45 wt%.
17. The heavy rare earth coating according to claim 16, characterized in that: The thickness of the heavy rare earth coating is 100nm~50μm.
18. A rare earth permanent magnet with a surface coated with a heavy rare earth composite coating, prepared by the method of any one of claims 1-15.
19. The application of the rare earth permanent magnet with a heavy rare earth composite coating as described in claim 18 in the diffusion of heavy rare earth grain boundaries.
Citation Information
Patent Citations
Electrodeposition method, electrodeposition solution and method for preparation of rare earth permanent magnetic material by electrodeposition
CN105839152A
Manufacturing method of permanent magnet material
CN106782980A
Treatment method for enhancing coercive force of neodymium-iron-boron magnet
CN115798914A