Solid-state lithium-sulfur battery alloy negative electrode, preparation method and application in solid-state lithium-sulfur battery
By using an alloy anode composed of metallic aluminum, doped elements, and lithium in lithium-sulfur batteries, the problems of lithium dendrite growth and slow lithium-ion transport have been solved, resulting in solid-state lithium-sulfur batteries with high energy density and high cycle efficiency.
Patent Information
- Application Number
- CN202311502052.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-13
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-13
AI Technical Summary
Existing lithium-sulfur battery alloy anodes are prone to lithium dendrite growth under high current density, resulting in poor lithium-ion transport performance, low battery cycle efficiency, and difficulty in meeting the requirements of high energy density and safety performance.
An alloy anode is formed by using metallic aluminum, doped elements, and metallic lithium. The doped elements are gallium, tin, germanium, or phosphorus. The alloy anode is formed by high-temperature calcination and rolling, which improves the lithium-ion conductivity and diffusion coefficient, and forms a fast transport channel.
It achieves high-area-capacity solid-state lithium-sulfur batteries with no lithium dendrite growth at high current density, stable charge-discharge cycles, high energy density and high cycle efficiency, ensuring safe battery operation.
Smart Images

Figure CN117613197B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid-state lithium batteries, specifically relating to a solid-state lithium-sulfur battery alloy anode, its preparation method, and its application in solid-state lithium-sulfur batteries. Background Technology
[0002] With the continuous development and upgrading of new energy electric vehicles, the energy storage market has placed higher demands on the energy density and safety performance of lithium-ion batteries. However, at present, lithium batteries based on liquid electrolytes are insufficient to meet the requirements of future new energy electric vehicles for rechargeable batteries, both in terms of energy density and safety performance. Solid-state lithium-ion batteries, which use solid electrolytes instead of liquid electrolytes, can simultaneously meet the requirements of lithium batteries for energy density and safety stability. Among them, solid-state lithium-sulfur batteries are representative of high energy density batteries, and their ultra-high theoretical energy density makes them one of the most valuable high-energy-density battery systems for research.
[0003] To achieve high energy density in solid-state lithium-sulfur batteries, the areal capacity of the sulfur cathode needs to reach 4 mAh / cm². 2 That's all. Furthermore, compared to traditional lithium-ion batteries, lithium-sulfur batteries have lower charge and discharge voltages. Therefore, at the same power density, lithium-sulfur batteries require higher current densities to maintain operation. However, currently researched lithium metal anodes, lithium indium anodes, lithium silicon anodes, and lithium aluminum alloy anodes all struggle to avoid operating at high current densities (>6 mA / cm²). 2 The problem of lithium dendrite growth is a significant one. Furthermore, because alloy anodes are prone to pulverization and have slow internal ion transport, a large number of lithium ions, once alloyed, are difficult to release again, leading to severe lithium loss and significantly limiting battery cycle efficiency. The fundamental issue is that lithium ions do not diffuse easily within the electrode, resulting in excessively low local potentials and thus the risk of lithium dendrite growth. Therefore, effectively improving the lithium-ion transport performance within the alloy anode can achieve uniform embedding and deposition of lithium ions, enabling stable cycling of the alloy anode at high current densities. Summary of the Invention
[0004] The purpose of this invention is to provide a solid-state lithium-sulfur battery alloy anode, its preparation method, and its application in solid-state lithium-sulfur batteries.
[0005] To achieve the above objectives, the present invention adopts the following technical solution:
[0006] A solid-state lithium-sulfur battery alloy anode is composed of metallic aluminum, doped elements, and metallic lithium, wherein the mass ratio of aluminum, doped elements, and metallic lithium is 76-84:14-16:2-8.
[0007] The doping element is one of gallium (Ga), tin (Sn), germanium (Ge), and phosphorus (P).
[0008] The aluminum has a particle size of 1–8 micrometers, and the dopant has a particle size of 100–500 nanometers.
[0009] The lithium-ion conductivity of the alloy anode is 0.5–1.2 mS / cm, and the lithium-ion diffusion coefficient is 1.0–1.5 × 10⁻⁶. -6 cm 2 / s.
[0010] This invention also provides a method for preparing the above-mentioned solid lithium-sulfur battery alloy anode, the preparation steps of which are:
[0011] (1) Mix metallic aluminum with doped element powder to form a mixture;
[0012] (2) Place this mixture in a high-temperature furnace under inert gas protection for calcination, and after cooling, form a calcined mixture;
[0013] (3) The calcined mixture is rolled by a roller press to form a calcined mixture film;
[0014] (4) Finally, the lithium metal is rolled onto the calcined mixture film to obtain the alloy negative electrode.
[0015] The mixture is calcined in a high-temperature furnace at a temperature of 700–820°C for 2–5 hours.
[0016] The thickness of the calcined mixture film is 10–50 micrometers.
[0017] The present invention also provides a solid-state lithium-sulfur battery, comprising the aforementioned alloy negative electrode, a solid electrolyte, and a sulfur positive electrode, wherein the areal capacity ratio of the alloy negative electrode to the sulfur positive electrode is 1.1 to 1.5.
[0018] The solid electrolyte can be Li6PS5Cl, Li 10 GeP2S 12 Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 One of them.
[0019] The advantages and positive effects of this invention are:
[0020] This invention expands the ion transport channels within the aluminum lattice through element doping, effectively reducing the transport energy barrier for lithium ions within the lattice and achieving rapid lithium ion transport. This alloy anode is suitable for high areal capacities (>5.5 mAh / cm²). 2 The solid-state lithium-sulfur battery sulfur cathode, under high current density (>8 mA / cm²), exhibits sulfur content. 2During charge-discharge cycles, no lithium dendrites grow on the negative electrode, thus enabling the solid-state lithium-sulfur battery based on a high areal capacity sulfur cathode to achieve high energy density, high cycle efficiency, and safe operation without lithium dendrites during charge-discharge at high current densities. Attached Figure Description
[0021] Figure 1 The modified alloy (Li) provided in Example 1 of this invention 0.05 Al 0.8 Sn 0.15 The negative electrode obstruction is a tomographic scan of a solid lithium-sulfur battery after 500 cycles (the lower layer is the alloy negative electrode, and the upper layer is the sulfur positive electrode). Detailed Implementation
[0022] The technical solution of the present invention will be further described in detail below through embodiments and comparative examples. However, it should be understood that these embodiments are merely for more detailed explanation and should not be construed as limiting the present invention in any way.
[0023] Example 1
[0024] (1) Alloy anode composition: mass ratio of aluminum: doped element tin: lithium = 80:15:5.
[0025] (2) Alloy anode preparation process: First, in an argon-filled tube furnace, 80 grams of aluminum powder with a particle size of 3 micrometers and 15 grams of doped tin powder with a particle size of 200 nanometers were mixed evenly. This mixture was then placed in an argon-filled tube furnace and calcined at 750°C for 2 hours, followed by cooling to room temperature to form a calcined mixture. This calcined mixture was then rolled to 45 micrometers using a roller press to form a calcined mixture film. Finally, this calcined mixture film was rolled with 5 grams of lithium metal sheets to uniformly disperse the lithium metal sheets on the calcined mixture film, ultimately obtaining Li. 0.05 Al 0.8 Sn 0.15 The alloy anode was determined to have an areal capacity of 5.04 mAh / cm³. 2 The lithium-ion conductivity is 0.5 mS / cm, and the lithium-ion diffusion coefficient is 1.2 × 10⁻⁶. -6 cm 2 / s.
[0026] (3) Solid-state lithium-sulfur battery fabrication: A Li6PS5Cl solid electrolyte membrane with a thickness of 40 micrometers and an areal capacity of 4.5 mAh / cm² was prepared. 2 The sulfur cathode (alloy anode surface capacity / sulfur cathode surface capacity = 1.12) and the alloy anode obtained in step (2) above are stacked together with Li6PS5Cl and sulfur cathode to form a multilayer solid-state lithium-sulfur soft-pack battery, and left to stand for 24 hours.
[0027] (4) Solid-state lithium-sulfur battery performance: The solid-state lithium-sulfur battery was tested and found to perform at 5 mA / cm². 2 The energy density is 410 Wh / kg at the current density and at 8 mA / cm². 2 After 500 continuous charge-discharge cycles at the current density, the capacity retention was 92%, and the average coulombic efficiency was 99.89%. Disassembly of the cycled battery revealed no lithium dendrite formation on the alloy negative electrode. (See attached image) Figure 1 ).
[0028] Example 2
[0029] The only difference from Example 1 is that in step (1), the mass ratio of aluminum:doped element tin:lithium is changed to 82:14:4, and the rest is the same as Example 1.
[0030] The areal capacity of this alloy anode was measured to be 5.2 mAh / cm³. 2 The lithium-ion conductivity is 0.45 mS / cm, and the lithium-ion diffusion coefficient is 1.02 × 10⁻⁶. -6 cm 2 / s.
[0031] Solid-state lithium-sulfur battery performance: Measurements showed that this solid-state lithium-sulfur battery achieved a speed of 5 mA / cm². 2 The energy density is 408 Wh / kg at the current density and at 8 mA / cm². 2 After 500 consecutive charge-discharge cycles at the current density, the capacity retention rate was 94%, and the average coulombic efficiency was 99.91%. Disassembly of the cycled battery revealed that no lithium dendrites were formed on the alloy negative electrode.
[0032] Example 3
[0033] The only difference from Example 1 is that in step (1), the mass ratio of aluminum:doped element tin:lithium is changed to 78:16:6, and the rest is the same as Example 1.
[0034] The areal capacity of this alloy anode was measured to be 4.9 mAh / cm³. 2 The lithium-ion conductivity is 0.42 mS / cm, and the lithium-ion diffusion coefficient is 0.96 × 10⁻⁶. -6 cm 2 / s.
[0035] Solid-state lithium-sulfur battery performance: Measurements showed that this solid-state lithium-sulfur battery achieved a speed of 5 mA / cm². 2 The energy density is 403 Wh / kg at the current density and at 8 mA / cm². 2 After 500 consecutive charge-discharge cycles at the current density, the capacity retention rate was 93%, and the average coulombic efficiency was 99.87%. Disassembly of the cycled battery revealed that no lithium dendrites were formed on the alloy negative electrode.
[0036] Example 4
[0037] The only difference from Example 1 is that in step (1), the mass ratio of aluminum: gallium dopant: lithium is changed to 81:15:4. The rest is the same as in Example 1.
[0038] The areal capacity of this alloy anode was measured to be 5.1 mAh / cm³. 2 The lithium-ion conductivity is 0.41 mS / cm, and the lithium-ion diffusion coefficient is 1.01 × 10⁻⁶. -6 cm 2 / s.
[0039] Solid-state lithium-sulfur battery performance: Measurements showed that this solid-state lithium-sulfur battery achieved a speed of 5 mA / cm². 2 The energy density is 404 Wh / kg at the current density and at 8 mA / cm². 2 After 500 consecutive charge-discharge cycles at the current density, the capacity retention rate was 91.5%, and the average coulombic efficiency was 99.86%. Disassembly of the cycled battery revealed that no lithium dendrites were formed on the alloy negative electrode.
[0040] Example 5
[0041] The only difference from Example 1 is that in step (1), the mass ratio of aluminum: gallium dopant: lithium is changed to 80:15:5, and the rest is the same as Example 1.
[0042] The areal capacity of this alloy anode was measured to be 5.2 mAh / cm³. 2 The lithium-ion conductivity is 0.42 mS / cm, and the lithium-ion diffusion coefficient is 1.05 × 10⁻⁶. -6 cm 2 / s.
[0043] Solid-state lithium-sulfur battery performance: Measurements showed that this solid-state lithium-sulfur battery achieved a speed of 5 mA / cm². 2 The energy density is 401 Wh / kg at the current density and at 8 mA / cm². 2 After 500 continuous charge-discharge cycles at the current density, the capacity retention rate was 89.5%, and the average coulombic efficiency was 99.85%. Disassembly of the cycled battery revealed that no lithium dendrites were formed on the alloy negative electrode.
[0044] Example 6
[0045] The only difference from Example 1 is that in step (1), the mass ratio of aluminum: gallium dopant: lithium is changed to 79:16:5, and the rest is the same as in Example 1.
[0046] The areal capacity of this alloy anode was measured to be 4.95 mAh / cm³. 2The lithium-ion conductivity is 0.43 mS / cm, and the lithium-ion diffusion coefficient is 1.07 × 10⁻⁶. -6 cm 2 / s.
[0047] Solid-state lithium-sulfur battery performance: Measurements showed that this solid-state lithium-sulfur battery achieved a speed of 5 mA / cm². 2 The energy density is 398 Wh / kg at the current density and at 8 mA / cm². 2 After 500 consecutive charge-discharge cycles at the current density, the capacity retention rate was 90.5%, and the average coulombic efficiency was 99.89%. Disassembly of the cycled battery revealed that no lithium dendrites were formed on the alloy negative electrode.
[0048] Example 7
[0049] The only difference from Example 1 is that in step (1), the mass ratio of aluminum: germanium: lithium is changed to 80:15:5. The rest is the same as in Example 1.
[0050] The areal capacity of this alloy anode was measured to be 5.2 mAh / cm³. 2 The lithium-ion conductivity is 0.54 mS / cm, and the lithium-ion diffusion coefficient is 1.24 × 10⁻⁶. -6 cm 2 / s.
[0051] Solid-state lithium-sulfur battery performance: Measurements showed that this solid-state lithium-sulfur battery achieved a speed of 5 mA / cm². 2 The energy density is 411 Wh / kg at the current density and at 8 mA / cm². 2 After 500 continuous charge-discharge cycles at the current density, the capacity retention rate was 92.5%, and the average coulombic efficiency was 99.92%. Disassembly of the cycled battery revealed that no lithium dendrites were formed on the alloy negative electrode.
[0052] Example 8
[0053] The only difference from Example 1 is that in step (1), the mass ratio of aluminum metal: dopant germanium: lithium metal is changed to 82:14:4, and the rest is the same as Example 1.
[0054] The areal capacity of this alloy anode was measured to be 5.2 mAh / cm³. 2 The lithium-ion conductivity is 0.51 mS / cm, and the lithium-ion diffusion coefficient is 1.14 × 10⁻⁶. -6 cm 2 / s.
[0055] Solid-state lithium-sulfur battery performance: Measurements showed that this solid-state lithium-sulfur battery achieved a speed of 5 mA / cm². 2 The energy density is 407 Wh / kg at the current density and at 8 mA / cm². 2After 500 continuous charge-discharge cycles at the current density, the capacity retention rate was 94.5%, and the average coulombic efficiency was 99.93%. Disassembly of the cycled battery revealed that no lithium dendrites were formed on the alloy negative electrode.
[0056] Comparative Example 1
[0057] The doping element tin was removed from Example 1, and the rest was the same as in Example 1.
[0058] Solid-state lithium-sulfur battery performance: Measurements showed that this solid-state lithium-sulfur battery achieved a speed of 5 mA / cm². 2 The energy density is 388 Wh / kg at the current density and at 8 mA / cm². 2 After eight consecutive charge-discharge cycles at the current density, the battery failed due to a short circuit. Disassembly of the cycled battery revealed a large number of lithium dendrites on the lithium-aluminum alloy negative electrode.
[0059] Comparative Example 2
[0060] The mass ratio of aluminum:doped tin:lithium in Example 1 was changed to 90:5:5, and the rest was the same as in Example 1.
[0061] Solid-state lithium-sulfur battery performance: Measurements showed that this solid-state lithium-sulfur battery achieved a speed of 5 mA / cm². 2 The energy density is 379 Wh / kg at the current density and at 8 mA / cm². 2 After 25 consecutive charge-discharge cycles at the current density, the battery failed due to a short circuit. Disassembly of the cycled battery revealed a large number of lithium dendrites on the lithium-aluminum alloy negative electrode.
[0062] Comparative Example 3
[0063] The mass ratio of aluminum:doped tin:lithium in Example 1 was changed to 75:20:5, and the rest was the same as in Example 1.
[0064] Solid-state lithium-sulfur battery performance: Measurements showed that this solid-state lithium-sulfur battery achieved a speed of 5 mA / cm². 2 The energy density is 405 Wh / kg at the current density and at 8 mA / cm². 2 After 38 consecutive charge-discharge cycles at the current density, the battery failed due to a short circuit. Disassembly of the cycled battery revealed a large number of lithium dendrites on the lithium-aluminum alloy negative electrode.
[0065] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A solid-state lithium-sulfur battery alloy anode, characterized in that: The alloy anode is composed of metallic aluminum, doped elements, and metallic lithium, with the mass ratio of metallic aluminum, doped elements, and metallic lithium being 84~76 : 14~16 : 2~8; the doped element is one of gallium (Ga), tin (Sn), germanium (Ge), and phosphorus (P).
2. The solid-state lithium-sulfur battery alloy anode according to claim 1, characterized in that: The aluminum has a particle size of 1-8 micrometers, and the dopant has a particle size of 100-500 nanometers.
3. A method for preparing a solid-state lithium-sulfur battery alloy anode as described in claim 1, characterized in that... It is made by the following steps: (1) Mix aluminum powder and doped element powder evenly to form a mixture; (2) Place this mixture in a high-temperature furnace under inert gas protection for calcination, and after cooling, form a calcined mixture; (3) The calcined mixture is rolled by a roller press to form a calcined mixture film; (4) Finally, the lithium metal is rolled onto the calcined mixture film to obtain the alloy negative electrode.
4. The solid-state lithium-sulfur battery alloy anode according to claim 3, characterized in that: In step (2), the calcination temperature of the mixture in the high-temperature furnace is 700~820℃, and the calcination time is 2~5 hours.
5. The solid-state lithium-sulfur battery alloy negative electrode according to claim 3, characterized in that: The thickness of the calcined mixture film is 10-50 micrometers.
6. A solid-state lithium-sulfur battery, comprising a negative electrode, a solid electrolyte, and a sulfur positive electrode, characterized in that: The negative electrode is the alloy negative electrode according to claim 1, wherein the areal capacity ratio of the alloy negative electrode to the sulfur positive electrode is 1.1 to 1.
5.
7. The solid-state lithium-sulfur battery according to claim 6, characterized in that: The solid electrolyte is Li6PS5Cl, Li 10 GeP2S 12 Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 One of them.
Citation Information
Patent Citations
Solid-state battery
CN113224377A
Preparation method of all-solid-state lithium battery taking lithium-aluminum alloy as negative electrode
CN114665068A
Aluminum-based negative pole piece for lithium ion battery and lithium ion secondary battery
CN114976037A