Preparation method of porous interlayer material for lithium-sulfur battery and application thereof
By preparing porous carbon nanofiber sandwich materials and utilizing cobalt and nitrogen-doped porous carbon structures, the shuttle effect problem of lithium polysulfides in lithium-sulfur batteries was solved, thereby improving the electrochemical performance and cycle capacity of the batteries.
Patent Information
- Application Number
- CN202311579813.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-24
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-11-24
AI Technical Summary
The shuttle effect of lithium polysulfides in lithium-sulfur batteries and the insufficient pure physical adsorption of lithium polysulfides by carbon materials result in low battery cycle capacity.
Carbon nanofibers were prepared by electrospinning and doped with cobalt and nitrogen to form a porous sandwich material. Combined with ZIF-67, the carbon was converted into cobalt-modified nitrogen-doped carbon, providing physical and chemical adsorption sites and mitigating the shuttle effect of lithium polysulfides.
It improves the electrochemical performance and specific capacity of lithium-sulfur batteries, enhances the adsorption capacity for lithium polysulfides, and extends the cycle life of the batteries.
Smart Images

Figure CN117613202B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-sulfur battery technology, specifically relating to a method for preparing porous sandwich materials for lithium-sulfur batteries and their applications. Background Technology
[0002] In recent years, humanity has begun to focus on renewable and clean energy sources, such as wind and solar power, hoping to solve problems such as energy depletion and environmental pollution. However, these clean energy sources have certain environmental requirements in practical applications and can also create an imbalance between power supply and demand. Therefore, it is necessary to find a new type of energy storage device to effectively convert, store, and utilize them.
[0003] Recently, researchers have focused their attention on rechargeable batteries. Among the many rechargeable batteries in use, such as nickel-cadmium, lead-acid, and lithium-ion batteries, lithium-ion batteries have become a research hotspot due to their high energy density, high operating voltage, and long cycle life. Traditional lithium-ion battery cathode materials, such as transition metal oxides (LiFeO2), are expensive and cause serious environmental pollution. Their low theoretical specific capacity of only 170 mAh / g cannot meet the demand for high energy density. Therefore, developing rechargeable battery systems with high energy density, low environmental pollution, and low cost has become an urgent research priority. Lithium-sulfur batteries have a high theoretical specific capacity (1675 mAh / g) and theoretical specific energy (2600 mAh / g), are relatively abundant on Earth, are inexpensive, and non-toxic, making them one of the most promising products for new electrochemical energy storage devices and a popular research area for international researchers.
[0004] However, the practical application of lithium-sulfur batteries is still constrained by many problems, such as the shuttle effect of intermediate lithium polysulfides and the poor conductivity of sulfur. Adding a conductive material as an interlayer between the battery cathode and the separator has proven to be an effective strategy, as it can provide a physical barrier to prevent the shuttle of polysulfides.
[0005] In recent years, various carbon-based battery interlayers with ideal porous structures have been developed. These carbon-based materials include carbon nanofibers (CNFs), carbon nanosheets, carbon nanotubes (CNTs), and graphene. These materials possess excellent conductivity and high specific surface area, which can physically confine lithium-ion migration. However, the non-polar nature of carbon materials means they can only physically adsorb lithium polysulfides, failing to provide strong chemisorption capacity for polar lithium ions, resulting in low battery cycle capacity. Therefore, introducing heteroatom doping and metal-based compounds into carbon-based interlayers to increase their polarity is a viable strategy. Polar materials can enhance the chemical capture of lithium ions, thereby suppressing the shuttle effect and significantly reducing the loss of active materials. Summary of the Invention
[0006] This invention provides a method for preparing a porous sandwich material for lithium-sulfur batteries and its application. Compared with existing technologies, the prepared porous sandwich material has high conductivity, stable electrochemical performance, high specific capacity, and can mitigate the shuttle effect in lithium-sulfur batteries.
[0007] To achieve the above objectives, the technical solution of the present invention includes the following steps: (1) Dissolve the pore-forming agent, cobalt salt, and carbon source in N,N-dimethylformamide to obtain a spinning precursor solution; (2) The spinning precursor solution is electrospinned to obtain fiber mat; (3) Dry the fiber felt at 60-80℃ for 5-6 hours, and calcine it in air at 200-300℃ to obtain carbon nanofibers; (4) Mix the aqueous solutions of cobalt salt, hexadecyltrimethylammonium bromide and dimethylimidazole, stir and react at room temperature for 30-60 min, seal and let stand for 12-24 h, centrifuge, wash the precipitate with distilled water and ethanol in sequence until the washing liquid is clear, dry the solid at 60-80℃ for 12-24 h to obtain ZIF-67 powder. (5) The carbon nanofibers obtained in step (3) are sequentially dipped into a suspension of polystyrene spheres and cobalt salt, and an ethanol suspension of ZIF-67, and dried at a constant temperature of 60-80℃ for 2-4 hours to obtain the precursor; (6) The precursor is calcined in a protective gas atmosphere to obtain a porous sandwich material for lithium-sulfur batteries.
[0008] Preferably, the cobalt salt is cobalt acetate or cobalt nitrate; Preferably, in step (1), the pore-forming agent is one of polystyrene, polymethyl methacrylate, and polyurethane, the carbon source is one of polyacrylonitrile, polyvinyl alcohol, and polyimide, the mass ratio of cobalt salt, carbon source, and pore-forming agent is 0.1-0.3:1:0.5-1, and the mass ratio of pore-forming agent to N,N-dimethylformamide is 0.06-0.1:1; Preferably, in step (4), the molar ratio of hexadecyltrimethylammonium bromide to cobalt salt is 1:20-30, the concentration of the cobalt salt aqueous solution is 0.05-0.15 mol / L, the concentration of the dimethylimidazole aqueous solution is 0.5-1 mol / L, and the molar ratio of cobalt salt to dimethylimidazole is 1:23-140. Preferably, in step (5), in the suspension of polystyrene spheres and cobalt salt, the concentration of cobalt salt is 0.15-0.2 mol / L, the mass percentage of polystyrene spheres is 0.99%-3%, the diameter of polystyrene spheres is 200-300 nm, and in the ethanol suspension of ZIF-67, the mass percentage of ZIF-67 is 0.5%-1%. Preferably, in step (6), the protective gas is argon or nitrogen, the heating rate is 1-2℃ / min, the calcination temperature is 500-600℃, and the calcination time is 6-10h.
[0009] The application of the porous sandwich material for lithium-sulfur batteries described in this invention involves applying the porous sandwich material for lithium-sulfur batteries to the positive electrode sandwich layer.
[0010] The beneficial effects of this invention are as follows: 1. The porous sandwich material for lithium-sulfur batteries of the present invention functions as a sandwich between the separator and the positive electrode. After calcination in a protective atmosphere, ZIF-67 is transformed into cobalt-modified nitrogen-doped porous carbon (Co-NC), whose abundant pores can physically adsorb lithium polysulfides. The polar Co nanocatalyst and the electronegative nitrogen-doped carbon serve as chemisorption sites, playing a synergistic role in the adsorption of polysulfides and mitigating the shuttle effect. Furthermore, the use of CNF, which is flexible and electrolyte-friendly, as the sandwich material substrate effectively improves the mechanical strength and electrolyte wettability of the sandwich material.
[0011] 2. The porous sandwich material (3D Co-NC@CNF) for lithium-sulfur batteries prepared in this invention has a first-cycle discharge specific capacity of 1285.24-1296.32 mAh / g at a current density of 0.2 C, and a capacity of 1089.58-1096.03 mAh / g after 100 cycles, with a capacity retention rate of 85.3%-88.1%; the first-cycle discharge specific capacity at a current density of 1 C is 993.35-998.12 mAh / g, with a capacity retention rate of 87.3-89.1%. Attached Figure Description
[0012] Figure 1 This is a scanning electron microscope (SEM) image of the 3D Co-NC@CNF material in Example 1; Figure 2 The image shows a SEM image of the 3D Co-NC@CNF material in Example 2. Figure 3 Here is a SEM image of the sandwich material in Comparative Example 2; Figure 4 The image shows the X-ray photoelectron spectroscopy (XPS) spectrum of Co 2p in 3D Co-NC@CNF in Example 1. Figure 5 The cycling curve of 3D Co-NC@CNF at 0.2C in Example 1; Figure 6 The cyclic curve of 3D Co-NC@CNF at 1C in Example 1 is shown. Detailed Implementation
[0013] The present invention will be described in detail below through embodiments. Example 1
[0014] (1) Dissolve 1.5g of polymethyl methacrylate, 0.4g of cobalt acetate, and 2g of polyacrylonitrile in 20mL of N,N-dimethylformamide to obtain a spinning precursor solution. The mass ratio of cobalt salt, carbon source, and pore-forming agent is 0.2:1:0.75, and the mass ratio of pore-forming agent to N,N-dimethylformamide is 0.079:1. (2) The spinning precursor solution was placed in an electrospinning environment with a voltage of 10kV, a pushing speed of 0.0015mm / s, and a receiving distance of 15cm to obtain fiber mat. (3) The fiber felt was dried at 60°C for 5 hours and then calcined in air at 200°C to obtain carbon nanofibers; (4) Dissolve 2 mmol cobalt nitrate and 0.08 mmol hexadecyltrimethylammonium bromide in 20 mL of distilled water, and dissolve 0.11 mol dimethylimidazole in 140 mL of distilled water. Mix the two solutions and stir at room temperature for 30 min, then seal and let stand for 12 h. After centrifugation, wash the precipitate with distilled water and ethanol in sequence until the washings are clear. Dry the solid at 60 °C for 12 h to obtain ZIF-67 powder. The molar ratio of hexadecyltrimethylammonium bromide to cobalt nitrate is 1:24, the concentration of cobalt nitrate aqueous solution is 0.1 mol / L, the concentration of dimethylimidazole aqueous solution is 0.79 mol / L, and the molar ratio of cobalt salt to dimethylimidazole is 1:55. (5) Add 0.1g of polystyrene spheres and 0.311g of cobalt acetate to 10mL of water, and add 0.12g of ZIF-67 to 20mL of ethanol. Dip the carbon nanofibers obtained in step (3) into the two suspensions in sequence, and dry them at 60℃ for 4h to obtain the precursor. In the suspension of polystyrene spheres and cobalt salt, the concentration of cobalt acetate is 0.18mol / L, the mass percentage of polystyrene spheres is 0.99%, the diameter of polystyrene spheres is 200nm, and in the ethanol suspension of ZIF-67, the mass percentage of ZIF-67 is 0.6%. (6) The precursor was calcined at 1℃ / min to 500℃ for 10h under an argon atmosphere to obtain a porous sandwich material for lithium-sulfur batteries. Example 2
[0015] (1) Dissolve 1.9g polystyrene, 0.57g cobalt nitrate, and 1.9g polyvinyl alcohol in 20mL of N,N-dimethylformamide to obtain a spinning precursor solution. The mass ratio of cobalt salt, carbon source, and pore-forming agent is 0.3:1:1, and the mass ratio of pore-forming agent to N,N-dimethylformamide is 0.1:1. (2) The spinning precursor solution was placed in an electrospinning environment with a voltage of 9kV, a pushing speed of 0.0015mm / s, and a receiving distance of 12cm to obtain fiber mat. (3) The fiber felt was dried at 80°C for 5 hours and then calcined in air at 250°C to obtain carbon nanofibers; (4) Dissolve 1 mmol cobalt acetate and 0.5 mmol hexadecyltrimethylammonium bromide in 20 mL of distilled water, and dissolve 0.14 mol dimethylimidazole in 140 mL of distilled water. Mix the two solutions and stir at room temperature for 45 min. Seal and let stand for 12 h. After centrifugation, wash the precipitate with distilled water and ethanol in sequence until the washing liquid is clear. Dry the solid at 75 °C for 18 h to obtain ZIF-67 powder. The molar ratio of hexadecyltrimethylammonium bromide to cobalt acetate is 1:20, the concentration of cobalt acetate aqueous solution is 0.05 mol / L, the concentration of dimethylimidazole aqueous solution is 1 mol / L, and the molar ratio of cobalt salt to dimethylimidazole is 1:140. (5) Add 0.2g of polystyrene spheres and 0.266g of cobalt acetate to 10mL of water, and add 0.2g of ZIF-67 to 20mL of ethanol. Dip the carbon nanofibers obtained in step (3) into the two suspensions in sequence, and dry them at 80℃ for 2h to obtain the precursor. In the suspension of polystyrene spheres and cobalt salt, the concentration of cobalt acetate is 0.15mol / L, the mass percentage of polystyrene spheres is 1.96%, the diameter of polystyrene spheres is 300nm, and in the ethanol suspension of ZIF-67, the mass percentage of ZIF-67 is 0.99%. (6) The precursor was placed in a nitrogen atmosphere and calcined at 550°C at 1°C / min for 12 hours to obtain a porous sandwich material for lithium-sulfur batteries. Example 3
[0016] (1) Dissolve 2g of polyurethane, 0.25g of cobalt acetate, and 2.5g of polyimide in 25mL of N,N-dimethylformamide to obtain a spinning precursor solution. The mass ratio of cobalt salt, carbon source, and pore-forming agent is 0.1:1:0.8, and the mass ratio of pore-forming agent to N,N-dimethylformamide is 0.084:1. (2) The spinning precursor solution was placed in an electrospinning environment with a voltage of 12kV, a pushing speed of 0.002mm / s, and a receiving distance of 14cm to obtain fiber mat. (3) The fiber felt was dried at 60°C for 6 hours and then calcined in air at 300°C to obtain carbon nanofibers; (4) Dissolve 2.4 mmol cobalt nitrate and 0.096 mmol hexadecyltrimethylammonium bromide in 20 mL of distilled water, and dissolve 0.084 mol dimethylimidazole in 140 mL of distilled water. Mix the two solutions and stir at room temperature for 60 min. Seal and let stand for 18 h. After centrifugation, wash the precipitate with distilled water and ethanol in sequence until the washing liquid is clear. Dry the solid at 80 °C for 24 h to obtain ZIF-67 powder. The molar ratio of hexadecyltrimethylammonium bromide to cobalt nitrate is 1:25, the concentration of cobalt nitrate aqueous solution is 0.12 mol / L, the concentration of dimethylimidazole aqueous solution is 0.6 mol / L, and the molar ratio of cobalt salt to dimethylimidazole is 1:35. (5) Add 0.31g of polystyrene spheres and 0.354g of cobalt acetate to 10mL of water, and add 0.15g of ZIF-67 to 20mL of ethanol. Dip the carbon nanofibers obtained in step (3) into the two suspensions in sequence, and dry them at 70℃ for 3h to obtain the precursor. In the suspension of polystyrene spheres and cobalt salt, the concentration of cobalt acetate is 0.2mol / L, the mass percentage of polystyrene spheres is 3%, the diameter of polystyrene spheres is 200nm, and in the ethanol suspension of ZIF-67, the mass percentage of ZIF-67 is 0.74%. (6) The precursor was placed in a nitrogen atmosphere and heated to 600 °C at 2 °C / min for 8 h to obtain a porous sandwich material for lithium-sulfur batteries. Example 4
[0017] (1) Dissolve 1.42g polystyrene, 0.852g cobalt nitrate, and 2.84g polyacrylonitrile in 25mL of N,N-dimethylformamide to obtain a spinning precursor solution. The mass ratio of cobalt salt, carbon source, and pore-forming agent is 0.3:1:0.5, and the mass ratio of pore-forming agent to N,N-dimethylformamide is 0.06:1. (2) The spinning precursor solution was placed in an electrospinning environment with a voltage of 6kV, a pushing speed of 0.001mm / s, and a receiving distance of 16cm to obtain fiber mat. (3) The fiber felt was dried at 70°C for 5.5 h and then calcined in air at 250°C to obtain carbon nanofibers; (4) Dissolve 3 mmol cobalt acetate and 0.1 mmol hexadecyltrimethylammonium bromide in 20 mL of distilled water, and dissolve 0.07 mol dimethylimidazole in 140 mL of distilled water. Mix the two solutions and stir at room temperature for 50 min. Seal and let stand for 24 h. After centrifugation, wash the precipitate with distilled water and ethanol in sequence until the washing liquid is clear. Dry the solid at 70 °C for 18 h to obtain ZIF-67 powder. The molar ratio of hexadecyltrimethylammonium bromide to cobalt acetate is 1:30, the concentration of cobalt acetate aqueous solution is 0.15 mol / L, the concentration of dimethylimidazole aqueous solution is 0.5 mol / L, and the molar ratio of cobalt salt to dimethylimidazole is 1:23. (5) Add 0.31g of polystyrene spheres and 0.329g of cobalt nitrate to 10mL of water, and add 0.12g of ZIF-67 to 20mL of ethanol. Dip the carbon nanofibers obtained in step (3) into the two suspensions in sequence, and dry them at 80℃ for 2h to obtain the precursor. In the suspension of polystyrene spheres and cobalt salt, the concentration of cobalt acetate is 0.18mol / L, the mass percentage of polystyrene spheres is 3%, the diameter of polystyrene spheres is 250nm, and in the ethanol suspension of ZIF-67, the mass percentage of ZIF-67 is 0.6%. (6) The precursor was placed in a nitrogen atmosphere and calcined at 1℃ / min to 550℃ for 12h to obtain a porous sandwich material for lithium-sulfur batteries. Comparative Example 1
[0018] This comparative example does not include polystyrene spheres. (1) Dissolve 1.5g of polymethyl methacrylate, 0.4g of cobalt acetate, and 2g of polyacrylonitrile in 20mL of N,N-dimethylformamide to obtain a spinning precursor solution. The mass ratio of cobalt salt, carbon source, and pore-forming agent is 0.2:1:0.75, and the mass ratio of pore-forming agent to N,N-dimethylformamide is 0.079:1. (2) The spinning precursor solution was placed in an electrospinning environment with a voltage of 10kV, a pushing speed of 0.0015mm / s, and a receiving distance of 15cm to obtain fiber mat. (3) The fiber felt was dried at 60°C for 5 hours and then calcined in air at 200°C to obtain carbon nanofibers; (4) Dissolve 2 mmol cobalt nitrate and 0.08 mmol hexadecyltrimethylammonium bromide in 20 mL of distilled water, and dissolve 0.11 mol dimethylimidazole in 140 mL of distilled water. Mix the two solutions and stir at room temperature for 30 min, then seal and let stand for 12 h. After centrifugation, wash the precipitate with distilled water and ethanol in sequence until the washings are clear. Dry the solid at 60 °C for 12 h to obtain ZIF-67 powder. The molar ratio of hexadecyltrimethylammonium bromide to cobalt nitrate is 1:24, the concentration of cobalt nitrate aqueous solution is 0.1 mol / L, the concentration of dimethylimidazole aqueous solution is 0.79 mol / L, and the molar ratio of cobalt salt to dimethylimidazole is 1:55. (5) Add 0.311g cobalt acetate to 10mL of water and 0.12g ZIF-67 to 20mL of ethanol. Dip the carbon nanofibers obtained in step (3) into the two solutions in sequence, and then dry them at 60℃ for 4h to obtain the precursor. The concentration of cobalt acetate is 0.18mol / L and the mass percentage of ZIF-67 is 0.6%. (6) The precursor was calcined at 500°C at 1°C / min for 10 h under an argon atmosphere to obtain the lithium-sulfur battery interlayer material. Comparative Example 2
[0019] This comparative example does not include ZIF-67. (1) Dissolve 1.5g of polymethyl methacrylate, 0.4g of cobalt acetate, and 2g of polyacrylonitrile in 20mL of N,N-dimethylformamide to obtain a spinning precursor solution. The mass ratio of cobalt salt, carbon source, and pore-forming agent is 0.2:1:0.75, and the mass ratio of pore-forming agent to N,N-dimethylformamide is 0.079:1. (2) The spinning precursor solution was placed in an electrospinning environment with a voltage of 10kV, a pushing speed of 0.0015mm / s, and a receiving distance of 15cm to obtain fiber mat. (3) The fiber felt was dried at 60°C for 5 hours and then calcined in air at 200°C to obtain carbon nanofiber fiber felt. (4) Add 0.12g of polystyrene spheres and 0.311g of cobalt acetate to 10mL of water. Dip the carbon nanofibers obtained in step (3) into the suspension and then dry them at 60℃ for 4h to obtain the precursor. The concentration of cobalt acetate is 0.18mol / L, the mass percentage of polystyrene spheres is 1.18%, and the size of polystyrene spheres is 200nm. (5) The precursor was calcined at 1℃ / min to 500℃ for 10h under an argon atmosphere to obtain lithium-sulfur battery interlayer material.
[0020] By comparison Figure 1 and Figure 2It can be observed that Example 1 and Example 2 have similar morphologies, while Figure 3 Unlike the previous two. Through Figure 3 We can see that CNF acts as a carrier, providing both conductivity and support. After being treated and calcined in a polystyrene ball suspension, the polystyrene ball template decomposes into a uniform macroporous structure, which covers the CNF and forms a conductive network with a porous structure, thereby increasing the specific surface area. Figure 1 and Figure 2 The morphology of 3D Co-NC@CNF is shown. After pyrolysis, ZIF-67 is distributed on macropores, and macropores are loaded on CNF, thus forming a multi-level structure. This structure improves conductivity and facilitates ion transport. On the other hand, it fixes lithium polysulfides from both physical and chemical perspectives, reducing the shuttle effect.
[0021] Figure 4 The Co2p spectrum of Example 1 shows four peaks at 780.9, 786.9, 797.3, and 803.9 eV, which are attributed to Co2p. 3 / 2 Co2p 1 / 2 And its corresponding satellite peaks.
[0022] Table 1
[0023] Table 1 above shows the discharge specific capacity of different samples; all examples and comparative examples were assembled into CR2032 button cells, and the entire process was carried out in an argon-filled glove box (H2O and O2 content less than 0.01 ppm). CNT / S was selected as the positive electrode material for lithium-sulfur batteries, and the interlayer material was placed between the electrode and the separator. Figure 5 The cycling curve of Example 1 at 0.2C shows that the initial discharge specific capacity is the highest at 1285.24 mAh / g, and the capacity retention rate is 85.3% after 100 cycles. Figure 6 The cycling curve of Example 1 at 1C shows that its initial discharge specific capacity was the highest at 993.65 mAh / g, and the capacity retention rate after 500 cycles was 89.1%. As shown in Table 1, the examples all exhibited the highest discharge specific capacity at different current densities with little difference. This indicates that the porous structure helps to fix polysulfides and permeate the electrolyte. At the same time, both Co and nitrogen-doped carbon can promote the conversion of lithium polysulfides, synergistically improving the performance of lithium-sulfur batteries.
[0024] The above embodiments are intended to illustrate the essential content of the present invention, but are not intended to limit the scope of protection of the present invention. Those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of protection of the present invention.
Claims
1. A method for preparing a porous sandwich material for lithium-sulfur batteries, characterized in that, Includes the following steps: (1) Dissolve the pore-forming agent, cobalt salt, and carbon source in N,N-dimethylformamide to obtain a spinning precursor solution; (2) The spinning precursor solution is electrospinned to obtain fiber mat; (3) Dry the fiber felt at 60-80℃ for 5-6 hours, and calcine it in air at 200-300℃ to obtain carbon nanofibers; (4) Mix the aqueous solutions of cobalt salt, hexadecyltrimethylammonium bromide and dimethylimidazole, stir and react at room temperature for 30-60 min, seal and let stand for 12-24 h, centrifuge, wash the precipitate with distilled water and ethanol in sequence until the washing liquid is clear, dry the solid at 60-80℃ for 12-24 h to obtain ZIF-67 powder. (5) The carbon nanofibers obtained in step (3) are sequentially dipped into a suspension of polystyrene spheres and cobalt salt, and an ethanol suspension of ZIF-67, and dried at a constant temperature of 60-80℃ for 2-4 hours to obtain the precursor; (6) The precursor is calcined in a protective gas atmosphere to obtain a porous sandwich material for lithium-sulfur batteries.
2. The method for preparing a porous sandwich material for lithium-sulfur batteries according to claim 1, characterized in that, The cobalt salt is cobalt acetate or cobalt nitrate.
3. The method for preparing a porous sandwich material for lithium-sulfur batteries according to claim 1, characterized in that, In step (1), the pore-forming agent is one of polystyrene, polymethyl methacrylate, and polyurethane, the carbon source is one of polyacrylonitrile, polyvinyl alcohol, and polyimide, the mass ratio of cobalt salt, carbon source, and pore-forming agent is 0.1-0.3:1:0.5-1, and the mass ratio of pore-forming agent to N,N-dimethylformamide is 0.06-0.1:
1.
4. The method for preparing a porous sandwich material for lithium-sulfur batteries according to claim 1, characterized in that, In step (4), the molar ratio of hexadecyltrimethylammonium bromide to cobalt salt is 1:20-30, the concentration of cobalt salt aqueous solution is 0.05-0.15 mol / L, the concentration of dimethylimidazole aqueous solution is 0.5-1 mol / L, and the molar ratio of cobalt salt to dimethylimidazole is 1:23-140.
5. The method for preparing a porous sandwich material for lithium-sulfur batteries according to claim 1, characterized in that, In step (5), the concentration of cobalt salt in the suspension of polystyrene spheres and cobalt salt is 0.15-0.2 mol / L, the mass percentage of polystyrene spheres is 0.99%-3%, the diameter of polystyrene spheres is 200-300 nm, and the mass percentage of ZIF-67 in the ethanol suspension of ZIF-67 is 0.5%-1%.
6. The method for preparing a porous sandwich material for lithium-sulfur batteries according to claim 1, characterized in that, In step (6), the protective gas is argon or nitrogen, the heating rate is 1-2℃ / min, the calcination temperature is 500-600℃, and the calcination time is 8-12h.
7. An application of a porous sandwich material for lithium-sulfur batteries obtained by the preparation method according to any one of claims 1-5, characterized in that, The aforementioned porous sandwich material for lithium-sulfur batteries is applied to the positive electrode sandwich of lithium-sulfur batteries.
Citation Information
Patent Citations
Method for preparing lithium-sulfur battery composite positive electrode material by electrostatic spinning method and application of lithium-sulfur battery composite positive electrode material
CN109768250A
Sandwich independent positive electrode for inhibiting shuttle effect of lithium-sulfur battery and preparation method of sandwich independent positive electrode