A positive electrode material, a preparation method thereof, a positive electrode sheet, a lithium ion battery, and a power-using device
By coating Co and W into the cathode material, the problems of high initial DC internal resistance and rapid growth of NCA-type ternary materials are solved, achieving low initial DCR and low DCR growth rate, thus improving the safety performance and cycle stability of the battery.
Patent Information
- Application Number
- CN202311235940.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-09-22
AI Technical Summary
The initial DC internal resistance of NCA-type ternary materials is high and increases too rapidly, leading to a decline in battery safety performance and severe capacity decay.
By simultaneously coating Co and W into the cathode material to form a co-coating layer, lithium-nickel mixing and residual alkali content are reduced, thereby improving electrochemical performance.
It reduces the initial DC internal resistance and internal resistance growth rate of the battery, improves the battery's safety performance and cycle stability, and alleviates capacity decay.
Smart Images

Figure CN117613205B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery technology, and more specifically, to a cathode material and its preparation method, a cathode sheet, a lithium-ion battery, and an electrical device. Background Technology
[0002] Lithium-ion batteries are increasingly favored by the battery industry due to their advantages such as lightweight design, long lifespan, and clean and environmentally friendly characteristics. As a key material in lithium-ion batteries, the cathode material has always been a focus of research and development in the industry. Currently, cathode materials for lithium-ion batteries include lithium cobalt oxide, lithium iron phosphate, lithium manganese oxide, nickel-cobalt-manganese ternary materials, and nickel-cobalt-aluminum ternary materials (NCA). Among them, NCA-type ternary materials are the most promising lithium-ion cathode materials, combining the advantages of lithium cobalt oxide and lithium nickel oxide, featuring high capacity, good cycle performance, and low cost.
[0003] However, NCA-type ternary materials currently suffer from high initial DCR and excessively rapid DCR growth, which can affect battery safety performance and lead to severe capacity decay.
[0004] In view of this, the present invention is hereby proposed. Summary of the Invention
[0005] The first objective of this invention is to provide a cathode material, in which a battery has a low initial DCR and a low DCR growth rate, which can reduce battery heat generation, improve its safety performance, or alleviate capacity decay.
[0006] The second objective of this invention is to provide a method for preparing a cathode material that, by simultaneously coating Co and W, can reduce the DCR of a battery containing the cathode material and can reduce the lithium-nickel mixture or residual alkali content of the cathode material. The cathode material prepared by this method has excellent electrochemical performance.
[0007] A third objective of this invention is to provide a positive electrode that has excellent cycle stability.
[0008] A fourth objective of this invention is to provide a lithium-ion battery with excellent electrochemical performance.
[0009] The fifth objective of this invention is to provide an electrical appliance.
[0010] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted:
[0011] The present invention provides a positive electrode material, wherein the initial DC internal resistance of a battery containing the positive electrode material is ≤10mΩ, and the rate of increase of DC internal resistance of a battery containing the positive electrode material after 100 cycles is ≤143.5%.
[0012] The present invention also provides a method for preparing the aforementioned cathode material, comprising the following steps:
[0013] The cathode material is obtained by sintering a mixture of a matrix material, a Co-containing coating agent, and a W-containing coating agent.
[0014] The coating agent includes a Co-containing coating agent and a W-containing coating agent.
[0015] The present invention also provides a positive electrode sheet, comprising the aforementioned positive electrode material.
[0016] The present invention also provides a lithium-ion battery, including the aforementioned positive electrode sheet.
[0017] The present invention also provides an electrical device, including the aforementioned lithium-ion battery.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0019] (1) The cathode material provided by the present invention, when assembled into a battery, has a low initial DCR and a low DCR growth rate, which can reduce the heat generation of the battery, improve its safety performance, and alleviate capacity decay.
[0020] (2) The cathode material provided by the present invention reduces the initial DCR and DCR growth rate of the battery made therefrom by introducing Co and W elements in the coating layer, reduces the heat generation level of the battery, improves its safety performance, and improves cycle stability.
[0021] (3) The cathode material provided by the present invention can reduce the mixing of lithium ions and nickel ions and reduce the residual alkalinity of the material. Attached Figure Description
[0022] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0023] Figure 1 This is a test graph showing the capacity retention of the cathode material provided in Embodiment 1 of the present invention after 100 cycles at 25°C and 0.5C.
[0024] Figure 2 This is a SEM image of the cathode material provided in Embodiment 1 of the present invention. Detailed Implementation
[0025] The technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings and specific embodiments. However, those skilled in the art will understand that the embodiments described below are some embodiments of the present invention, but not all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall be followed. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0026] In a first aspect, the present invention provides a positive electrode material, wherein the initial DC internal resistance of a battery containing the positive electrode material is ≤10mΩ, including but not limited to a point value or a range between any two of 10mΩ, 9.9mΩ, 9.8mΩ, 9.7mΩ, 9.6mΩ, 9.5mΩ, 9.3mΩ, 9.1mΩ, and 9.0mΩ.
[0027] Furthermore, the rate of increase of DC internal resistance of a battery containing this positive electrode material after 100 cycles is ≤143.5%, including but not limited to any one of 143.5%, 143.4%, 143.2%, 143%, 142%, 141%, 140%, 138%, 135%, or any range between two of them.
[0028] The battery containing this cathode material provided by the present invention has a low initial DCR and a low DCR growth rate, thereby reducing the heat generation of the battery, improving its safety performance, and mitigating capacity decay.
[0029] In some specific embodiments, the battery containing the positive electrode material has a DC internal resistance ≤20mΩ after 100 cycles; including but not limited to the point value of any one of 20mΩ, 19.8mΩ, 19.6mΩ, 19.4mΩ, 19.2mΩ, and 19.0mΩ, or the range between any two.
[0030] In some specific embodiments, the battery containing the positive electrode material has a capacity retention rate of ≥96.5% after 100 cycles; including but not limited to any one of 96.5%, 96.8%, 97%, 97.2%, 97.5%, 97.8%, 98%, or any range between two of them.
[0031] The cathode material provided by this invention also exhibits excellent cycle stability when assembled into a battery.
[0032] The aforementioned battery containing positive electrode material includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte.
[0033] In some specific embodiments, the battery containing the positive electrode material is a CR2032 coin cell.
[0034] The active material used in the positive electrode is the aforementioned positive electrode material.
[0035] In some specific embodiments, the preparation method of the above-mentioned positive electrode sheet includes: mixing the positive electrode material with acetylene black and PVDF in a mass ratio of 90:4:6, coating it on an aluminum foil current collector, drying it at 100°C, rolling it, punching it into a disc with a diameter of 16mm using a punching machine, and vacuum drying it at 120°C for 12h to obtain the positive electrode sheet.
[0036] In some specific implementations, the negative electrode is a lithium sheet.
[0037] In some specific embodiments, the electrolyte is a 1 mol / L LiPF6 EC+DMC+DEC solution.
[0038] In some specific embodiments, the diaphragm is a Celgard 2400 diaphragm.
[0039] In some specific implementations, a Wuhan LAND CT3001A charge-discharge tester was used to conduct electrochemical charge-discharge cycle tests on the aforementioned batteries containing positive electrode materials, with a voltage range of 2.5–4.25V (vs. Li). + / Li), with a current of 20mA / g, initial DC internal resistance (DCR) and 100-cycle DCR tests were performed at 100% SOC (fully charged).
[0040] In some specific implementations, the test methods for initial DCR and 100-cycle DCR are as follows: a fully charged battery is left to stand for 1 hour; the battery is adjusted to 100% SOC using a 1C current; the battery is left to stand for 30 minutes, and the voltage V0 at this time is recorded as the OCV at 100% SOC; the battery is discharged using a discharge current I1 for 60 seconds, and the voltage V1 at the 60th second is recorded; the formula for calculating the DC internal resistance during discharge is: DCR = (V0 - V1) / I1.
[0041] In some specific embodiments, the lithium-nickel mixing ratio of the cathode material is ≤2.0%; preferably ≤1.95%. The cathode material provided by the present invention also has a low lithium-nickel mixing ratio.
[0042] In some specific embodiments, the residual alkali content of the cathode material is ≤0.25%; preferably ≤0.248%. The cathode material provided by the present invention has a low residual alkali content.
[0043] In some specific embodiments, the aforementioned positive electrode material includes a matrix material and a coating layer covering the outer surface of the matrix material.
[0044] The chemical formula of the matrix material is Li a Ni 1-x-y-b Co x Al y M b O2; where 1≤a≤1.06, 0 <x≤0.1,0<y≤0.1,0≤b≤0.05。
[0045] M includes at least one of the elements Ga, W, Zr, B, Sb, Mo, Ti, La, and Sn.
[0046] The above chemical formula Li a Ni 1-x-y-b Co x Al y M b In O2, a includes, but is not limited to, any one of the values 1, 1.01, 1.02, 1.03, 1.04, 1.05, and 1.06, or any range between any two; x includes, but is not limited to, any one of the values 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, and 0.1, or any range between any two; y includes, but is not limited to, any one of the values 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, and 0.1, or any range between any two; b includes, but is not limited to, any one of the values 0, 0.01, 0.02, 0.03, 0.04, and 0.05, or any range between any two.
[0047] The coating layer includes Co and W elements.
[0048] In some specific embodiments, the coating layer comprises cobalt oxide and tungsten oxide.
[0049] The cathode material provided by this invention, through cobalt-tungsten co-coating modification, solves the problems of high initial DCR and excessively rapid DCR growth, which can reduce the heat generation level of the battery, improve its safety performance, and alleviate capacity decay.
[0050] The advantages of cobalt-tungsten co-coating are as follows: First, it reduces electrolyte corrosion during charging and discharging, decreasing metal ion dissolution and thus ensuring discharge capacity. Second, the cobalt-tungsten blended metal oxide coating can absorb HF, thereby improving cycle stability. Third, it can suppress lattice distortion to the greatest extent. All three points make it easier for lithium ions to shuttle between crystal lattices during charging and discharging, reducing impedance.
[0051] Furthermore, the Co element in the coating layer can improve cycle performance and stabilize the structure during charge and discharge, while reducing the mixing of lithium and nickel ions and lowering the residual basicity of the material. Therefore, the cathode material provided by this invention also solves the problem of conventional high-nickel NCA materials undergoing side reactions with water and carbon dioxide in the air during storage, producing electrochemically inert byproducts such as lithium hydroxide and lithium carbonate, which in turn affect electrochemical performance.
[0052] Furthermore, when element M is doped into the matrix material, the structure of the matrix material can be stabilized, thereby improving the cycle efficiency of the battery made from it.
[0053] In some specific embodiments, the thickness of the coating layer is 2 to 4 nm, including but not limited to a point value of any one of 2 nm, 2.5 nm, 3 nm, 3.5 nm, and 4 nm, or a range between any two.
[0054] Using a coating layer within this thickness range helps reduce electrolyte corrosion and surface side reactions.
[0055] In some specific embodiments, the molar ratio of Co element in the coating layer to the matrix material is 0.01 to 0.015:1, for example 0.010:1, 0.011:1, 0.012:1, 0.013:1, 0.014:1 or 0.015:1.
[0056] In some specific embodiments, the molar ratio of W element in the coating layer to the matrix material is 0.01 to 0.015:1, for example, 0.010:1, 0.011:1, 0.012:1, 0.013:1, 0.014:1 or 0.015:1.
[0057] In some specific embodiments, the molar ratio of Co to W in the coating layer is 1:1.0 to 1.5, for example, 1:1.0, 1:1.1, 1:1.2, 1:1.3, 1:1.4 or 1:1.5.
[0058] Secondly, the present invention provides a method for preparing the aforementioned cathode material, comprising the following steps:
[0059] Li as the matrix material a Ni 1-x-y-b Co x Al y M b O2, a Co-containing coating agent, and a W-containing coating agent are mixed evenly and then sintered to obtain the cathode material.
[0060] The coating agent includes a Co-containing coating agent and a W-containing coating agent.
[0061] The method for preparing the cathode material provided by this invention can reduce the lithium-nickel mixing and residual alkali content of the cathode material by simultaneously coating Co and W, and reduce the DCR of the battery made from the cathode material. The cathode material prepared by this method has excellent electrochemical performance, good cycle stability and good safety performance after being made into a battery.
[0062] In addition, the above preparation method has the advantages of simple operation, short process and suitability for mass production.
[0063] In some specific embodiments, the Co-containing coating agent includes a Co-containing compound.
[0064] In some specific embodiments, the Co-containing compound includes one or more of the following: oxides, hydroxides, carbonates, and nitrates of Co.
[0065] In some specific embodiments, the W-containing coating agent includes a W-containing compound.
[0066] In some specific embodiments, the W-containing compound includes one or more of the following: oxides, hydroxides, carbonates, and nitrates of W.
[0067] In some specific embodiments, the sintering temperature is 500 to 700°C; including but not limited to any one of 500°C, 550°C, 600°C, 650°C, and 700°C, or a range between any two.
[0068] In some specific embodiments, the sintering holding time is 5 to 7 hours; including but not limited to any one of 5 hours, 5.5 hours, 6 hours, 6.5 hours, and 7 hours, or any range between two of them.
[0069] In some specific embodiments, the heating rate during the sintering process is 2 to 4 °C / min, including but not limited to any one of 2 °C / min, 2.5 °C / min, 3 °C / min, 3.5 °C / min, 4 °C / min, or any range between two of them.
[0070] In some specific embodiments, the sintering is carried out in an oxygen atmosphere.
[0071] In some specific embodiments, after sintering, a sieving (screening) step is also included.
[0072] In some specific embodiments, the matrix material is mainly prepared by calcining a mixture of nickel-cobalt hydroxide, a lithium source, and an aluminum source. When the mixture does not contain dopants, the chemical formula of the prepared matrix material has b = 0.
[0073] In some specific embodiments, the matrix material is mainly prepared by calcining a mixture of nickel-cobalt hydroxide, a lithium source, an aluminum source, and a dopant; wherein the doping element in the dopant includes at least one of Ga, W, Zr, B, Sb, Mo, Ti, La, and Sn. In this case, b is not equal to 0.
[0074] The chemical formula of nickel cobalt hydroxide is Ni 1-x Co x (OH)2.
[0075] In some specific embodiments, the dopant includes at least one of Ga-containing compounds, W-containing compounds, Zr-containing compounds, B-containing compounds, Sb-containing compounds, Mo-containing compounds, Ti-containing compounds, La-containing compounds, and Sn-containing compounds.
[0076] In some specific embodiments, the lithium source includes any conventional lithium-containing compound, such as at least one of lithium oxides, hydroxides or carbonates thereof, but is not limited thereto.
[0077] In some specific embodiments, the aluminum source includes, but is not limited to, any conventional aluminum-containing compound, such as at least one of aluminum oxides, hydroxides or carbonates thereof.
[0078] In some specific embodiments, the molar ratio of nickel cobalt hydroxide, lithium source, aluminum source and dopant is 1:1 to 1.06:0.01 to 0.1:0 to 0.05.
[0079] In some specific embodiments, the calcination is a two-stage calcination, specifically including the following steps: first, holding at 500-700℃ for 5-7 hours (referred to as the first stage), and then holding at 600-800℃ for 12-16 hours (referred to as the second stage).
[0080] This invention employs a two-stage calcination process. The first stage allows the lithium source to be initially melted, while the second stage allows the lithium source to fully react with nickel-cobalt hydroxide, thereby increasing the material's capacity.
[0081] The calcination temperature in the first stage includes, but is not limited to, any one of 500℃, 530℃, 550℃, 580℃, 600℃, 620℃, 650℃, and 680℃, or any range between any two; the holding time in the first stage includes, but is not limited to, any one of 5h, 5.5h, 6h, 6.5h, and 7h, or any range between any two.
[0082] The calcination temperature in the second stage includes, but is not limited to, any one of 600℃, 620℃, 650℃, 680℃, 700℃, 720℃, 740℃, 750℃, 760℃, 780℃, and 800℃, or any range between two of them; the holding time in the second stage includes, but is not limited to, any one of 12h, 13h, 14h, 15h, and 16h, or any range between two of them.
[0083] In some specific implementations, the heating rate during the calcination process is 2–4 °C / min.
[0084] In some specific embodiments, during the calcination process, nickel-cobalt hydroxide, lithium source and aluminum source are mixed and then placed into a sagger for sintering, with the height of the mixture in the sagger being 4 to 6 cm.
[0085] In some specific implementations, calcination is carried out in an oxygen atmosphere.
[0086] In some specific implementations, the calcined product is further crushed and sieved.
[0087] In some specific embodiments, the median particle size D50 of the matrix material is 10 to 12 μm, for example, 10 μm, 11 μm or 12 μm.
[0088] In some specific embodiments, the median particle size D50 of the Co-containing coating agent and / or the W-containing coating agent is 40–50 μm, for example 40 μm, 43 μm, 45 μm, 48 μm or 50 μm.
[0089] In some specific embodiments, the median particle size D50 of the cathode material is 10–12 μm, for example, 10 μm, 11 μm or 12 μm.
[0090] Thirdly, the present invention provides a positive electrode sheet comprising the positive electrode material as described above.
[0091] In some specific embodiments, the positive electrode sheet includes a current collector and a positive electrode material coated on the current collector, wherein the positive electrode material is mainly composed of the aforementioned positive electrode material, a binder, and a conductive agent.
[0092] The binder can be any commercially available material with a binding effect that can be used to make the positive electrode sheet, such as polyvinylidene fluoride (PVDF), but is not limited to this.
[0093] The conductive agent can be any commercially available battery conductive agent, such as graphite, carbon black, and conductive polymers, but is not limited to these.
[0094] Fourthly, the present invention provides a lithium-ion battery, including the positive electrode sheet as described above.
[0095] In some specific implementations, lithium-ion batteries also include a negative electrode, a separator, and an electrolyte.
[0096] The negative electrode includes any commercially available negative electrode or a negative electrode that can be made using any existing technology.
[0097] The diaphragm and electrolyte include any conventional diaphragm and electrolyte that can be purchased or made using any existing technology.
[0098] Fifthly, the present invention provides an electrical device including the lithium-ion battery described above.
[0099] It is understood that the aforementioned electrical equipment includes any device, apparatus, or system that uses the aforementioned lithium-ion battery.
[0100] For example, the aforementioned lithium-ion batteries can be applied in the fields of transportation, electronics, aerospace, medical, and energy storage, but are not limited to these.
[0101] The embodiments of the present invention will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be considered as limiting the scope of the invention. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer are followed. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.
[0102] Example 1
[0103] The cathode material provided in this embodiment includes a matrix material and a coating layer covering the surface of the matrix material. The matrix material has the chemical formula Li. 1.045 Ni 0.87 Co 0.1 Al 0.03 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.01:0.01:1. The thickness of the coating is 2.6 nm.
[0104] The method for preparing the cathode material provided in this embodiment includes the following steps:
[0105] (1) Ni cobalt hydroxide Ni 0.9 Co 0.1 After (OH)2, lithium hydroxide, and aluminum oxide are mixed evenly, a first mixture is obtained, wherein the molar ratio of lithium hydroxide to nickel cobalt manganese hydroxide is 1.045:1, and the molar ratio (i.e., the molar ratio) of aluminum in aluminum oxide to nickel cobalt hydroxide is 0.03:1. That is, x = 0.1, a = 1.045, y = 0.03.
[0106] The first mixture was loaded into a sagger and placed in a kiln for calcination in an oxygen atmosphere. The height of the first mixture in the sagger was 5 cm. The calcination was divided into two stages: the first stage calcination temperature was 580℃ and the holding time was 5 hours; the second stage calcination temperature was 740℃ and the holding time was 13 hours. The heating rate was 2.5℃ / min during both stages. After the holding time was completed, the material was cooled with the furnace. After cooling, the material was crushed and sieved to obtain the matrix material.
[0107] (2) The matrix material obtained in step (1) is mixed evenly with tungsten oxide and cobalt oxide to obtain a second mixture, wherein the molar ratio of tungsten, cobalt and matrix material is 0.01:0.01:1. The second mixture is placed in a sagger and then placed in a kiln for sintering in an oxygen atmosphere at a sintering temperature of 680℃ for 5 hours. The sintered material is then sieved to obtain the modified cathode material.
[0108] Example 2
[0109] The cathode material provided in this embodiment includes a matrix material and a coating layer covering the surface of the matrix material. The matrix material has the chemical formula Li. 1.045 Ni 0.87 Co 0.1 Al 0.03 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.01:0.012:1. The thickness of the coating is 2.7 nm.
[0110] The preparation method of the cathode material provided in this embodiment is basically the same as that in Example 1. The only difference is that in step (2), the molar ratio of tungsten, cobalt and matrix material is 0.01:0.012:1.
[0111] Example 3
[0112] The cathode material provided in this embodiment includes a matrix material and a coating layer covering the surface of the matrix material. The matrix material has the chemical formula Li. 1.045 Ni 0.87 Co 0.1 Al 0.03 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.01:0.015:1. The thickness of the coating is 2.8 nm.
[0113] The preparation method of the cathode material provided in this embodiment is basically the same as that in Example 1. The only difference is that in step (2), the molar ratio of tungsten, cobalt and matrix material is 0.01:0.015:1.
[0114] Example 4
[0115] The cathode material provided in this embodiment includes a matrix material and a coating layer covering the surface of the matrix material. The matrix material has the chemical formula Li. 1.045 Ni 0.87 Co 0.1 Al 0.03 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.015:0.012:1. The thickness of the coating is 3.0 nm.
[0116] The preparation method of the cathode material provided in this embodiment is basically the same as that in Example 1. The only difference is that in step (2), the molar ratio of tungsten, cobalt and matrix material is 0.015:0.012:1.
[0117] Example 5
[0118] The cathode material provided in this embodiment includes a matrix material and a coating layer covering the surface of the matrix material. The matrix material has the chemical formula Li. 1.045 Ni 0.83 Co 0.1 Al 0.03 Sb 0.04 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.01:0.01:1. The thickness of the coating is 2.6 nm.
[0119] The method for preparing the cathode material provided in this embodiment includes the following steps:
[0120] (1) Ni cobalt hydroxide Ni 0.9 Co 0.1 (OH)₂, lithium hydroxide, aluminum oxide, and antimony trioxide are mixed evenly to obtain a first mixture. The molar ratio of lithium hydroxide to nickel cobalt manganese hydroxide is 1.045:1, the molar ratio of aluminum in aluminum oxide to nickel cobalt hydroxide is 0.03:1, and the molar ratio of antimony in antimony trioxide to nickel cobalt hydroxide is 0.04:1. That is, x = 0.1, a = 1.045, y = 0.03, and b = 0.04.
[0121] The first mixture was loaded into a sagger and placed in a kiln for calcination in an oxygen atmosphere, with the same calcination parameters as in Example 1. After cooling, the material was crushed and sieved to obtain the matrix material.
[0122] (2) Same as step (2) in Example 1.
[0123] Example 6
[0124] The cathode material provided in this embodiment includes a matrix material and a coating layer covering the surface of the matrix material. The matrix material has the chemical formula Li. 1.02 Ni 0.87 Co 0.1 Al 0.02 B 0.01 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.01:0.01:1. The thickness of the coating is 2.6 nm.
[0125] The method for preparing the cathode material provided in this embodiment includes the following steps:
[0126] (1) Ni cobalt hydroxide Ni 0.9 Co 0.1 After (OH)₂, lithium hydroxide, aluminum oxide, and boron oxide are mixed evenly, a first mixture is obtained. The molar ratio of lithium hydroxide to nickel cobalt manganese hydroxide is 1.02:1, the molar ratio of aluminum in aluminum oxide to nickel cobalt hydroxide is 0.02:1, and the molar ratio of boron in boron oxide to nickel cobalt hydroxide is 0.01:1. That is, x = 0.1, a = 1.02, y = 0.02, and b = 0.01.
[0127] The first mixture was loaded into a sagger and placed in a kiln for calcination in an oxygen atmosphere. The height of the first mixture in the sagger was 5 cm. The calcination was divided into two stages: the first stage calcination temperature was 530℃, and the holding time was 5 hours; the second stage calcination temperature was 650℃, and the holding time was 15 hours. The heating rate was 2.5℃ / min during both stages. After the holding time was completed, the material was cooled with the furnace. After cooling, the material was crushed and sieved to obtain the matrix material.
[0128] (2) The matrix material obtained in step (1) is mixed evenly with tungsten oxide and cobalt oxide to obtain a second mixture, wherein the molar ratio of tungsten, cobalt and matrix material is 0.01:0.01:1. The second mixture is placed in a sagger and then placed in a kiln for sintering in an oxygen atmosphere at a sintering temperature of 600℃ for 6 hours. The sintered material is then sieved to obtain the modified cathode material.
[0129] Example 7
[0130] The cathode material provided in this embodiment includes a matrix material and a coating layer covering the surface of the matrix material. The matrix material has the chemical formula Li. 1.06 Ni 0.82 Co 0.08 Al 0.05 Ga 0.02 Ti0.03 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.01:0.01:1. The thickness of the coating is 2.3 nm.
[0131] The method for preparing the cathode material provided in this embodiment includes the following steps:
[0132] (1) Ni cobalt hydroxide Ni 0.92 Co 0.08 (OH)₂, lithium hydroxide, aluminum oxide, gallium oxide, and titanium oxide are mixed evenly to obtain a first mixture. The molar ratio of lithium hydroxide to nickel cobalt manganese hydroxide is 1.06:1; the molar ratio of aluminum in aluminum oxide to nickel cobalt hydroxide is 0.05:1; the molar ratio of gallium in gallium oxide to nickel cobalt hydroxide is 0.02:1; and the molar ratio of titanium in titanium oxide to nickel cobalt hydroxide is 0.03:1. That is, x = 0.08, a = 1.06, y = 0.05, and b = 0.05.
[0133] The first mixture was loaded into a sagger and placed in a kiln for calcination in an oxygen atmosphere. The height of the first mixture in the sagger was 5 cm. The calcination was divided into two stages: the first stage calcination temperature was 600℃ and the holding time was 6 hours; the second stage calcination temperature was 780℃ and the holding time was 14 hours. The heating rate was 2.5℃ / min during both stages. After the holding time was completed, the material was cooled with the furnace. After cooling, the material was crushed and sieved to obtain the matrix material.
[0134] (2) The matrix material obtained in step (1) is mixed evenly with tungsten oxide and cobalt oxide to obtain a second mixture, wherein the molar ratio of tungsten, cobalt and matrix material is 0.01:0.01:1. The second mixture is placed in a sagger and then placed in a kiln for sintering in an oxygen atmosphere at a sintering temperature of 580℃ for 6 hours. The sintered material is then sieved to obtain the modified cathode material.
[0135] Example 8
[0136] The cathode material provided in this embodiment includes a matrix material and a coating layer covering the surface of the matrix material. The matrix material has the chemical formula Li. 1.03 Ni 0.85 Co 0.05 Al 0.08 Zr 0.01 Mo 0.01 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.01:0.01:1. The thickness of the coating is 2.2 nm.
[0137] The method for preparing the cathode material provided in this embodiment includes the following steps:
[0138] (1) Ni cobalt hydroxide Ni 0.95 Co 0.05 (OH)₂, lithium hydroxide, aluminum oxide, zirconium dioxide, and molybdenum trioxide are mixed evenly to obtain a first mixture. The molar ratio of lithium hydroxide to nickel cobalt manganese hydroxide is 1.03:1; the molar ratio of aluminum in aluminum oxide to nickel cobalt hydroxide is 0.08:1; the molar ratio of zirconium in zirconium dioxide to nickel cobalt hydroxide is 0.01:1; and the molar ratio of molybdenum in molybdenum trioxide to nickel cobalt hydroxide is 0.01:1. That is, x = 0.05, a = 1.03, y = 0.08, and b = 0.02.
[0139] The first mixture was loaded into a sagger and placed in a kiln for calcination in an oxygen atmosphere. The height of the first mixture in the sagger was 5 cm. The calcination was divided into two stages: the first stage calcination temperature was 650℃ and the holding time was 5 hours; the second stage calcination temperature was 800℃ and the holding time was 12 hours. The heating rate was 4℃ / min during both stages. After the holding time was completed, the material was cooled with the furnace. After cooling, the material was crushed and sieved to obtain the matrix material.
[0140] (2) The matrix material obtained in step (1) is mixed evenly with tungsten oxide and cobalt oxide to obtain a second mixture, wherein the molar ratio of tungsten, cobalt and matrix material is 0.01:0.01:1. The second mixture is placed in a sagger and then placed in a kiln for sintering in an oxygen atmosphere at a sintering temperature of 550℃ for 6.5h. The sintered material is then sieved to obtain the modified cathode material.
[0141] Example 9
[0142] The cathode material provided in this embodiment includes a matrix material and a coating layer covering the surface of the matrix material. The matrix material has the chemical formula Li. 1.045 Ni 0.82 Co 0.1 Al 0.03 Sn 0.03 W 0.02 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.01:0.01:1. The thickness of the coating is 2.4 nm.
[0143] The method for preparing the cathode material provided in this embodiment includes the following steps:
[0144] (1) Ni cobalt hydroxide Ni 0.9 Co0.1 (OH)₂, lithium hydroxide, aluminum oxide, tin oxide, and tungsten oxide are mixed evenly to obtain a first mixture. The molar ratio of lithium hydroxide to nickel cobalt manganese hydroxide is 1.045:1; the molar ratio of aluminum in aluminum oxide to nickel cobalt hydroxide is 0.03:1; the molar ratio of tin in tin oxide to nickel cobalt hydroxide is 0.03:1; and the molar ratio of tungsten in tungsten oxide to nickel cobalt hydroxide is 0.02:1. That is, x = 0.1, a = 1.045, y = 0.03, and b = 0.05.
[0145] The first mixture was placed in a sagger and then calcined in an oxygen atmosphere in a kiln. The height of the first mixture in the sagger was 5 cm. The calcination was divided into two stages: the first stage calcination temperature was 700℃ and the holding time was 5 hours; the second stage calcination temperature was 750℃ and the holding time was 12 hours. The heating rate was 3℃ / min during both stages. After the holding time was completed, the material was cooled with the furnace. After cooling, the material was crushed and sieved to obtain the matrix material.
[0146] (2) The matrix material obtained in step (1) is mixed evenly with tungsten oxide and cobalt oxide to obtain a second mixture, wherein the molar ratio of tungsten, cobalt and matrix material is 0.01:0.01:1. The second mixture is placed in a sagger and then placed in a kiln for sintering in an oxygen atmosphere at a sintering temperature of 530℃ for 7 hours. The sintered material is then sieved to obtain the modified cathode material.
[0147] Example 10
[0148] The cathode material provided in this embodiment includes a matrix material and a coating layer covering the surface of the matrix material. The matrix material has the chemical formula Li. 1.045 Ni 0.87 Co 0.1 Al 0.03 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.015:0.015:1. The thickness of the coating is 3.2 nm.
[0149] The preparation method of the cathode material provided in this embodiment is basically the same as that in Example 1. The only difference is that in step (2), the molar ratio of tungsten, cobalt and matrix material is 0.015:0.015:1.
[0150] Comparative Example 1
[0151] The cathode material provided in this comparative example includes a substrate material and a coating layer covering the surface of the substrate material. The substrate material has the chemical formula Li. 1.045 Ni 0.87Co 0.1 Al 0.03 The coating material is cobalt oxide, with O2. The molar ratio of Co to the matrix material in the coating is 0.01:1. The thickness of the coating is 1.5 nm.
[0152] The preparation method of the cathode material provided in this comparative example is basically the same as that in Example 1, except that tungsten oxide is not added in step (2).
[0153] Comparative Example 2
[0154] The cathode material provided in this comparative example includes a substrate material and a coating layer covering the surface of the substrate material. The substrate material has the chemical formula Li. 1.045 Ni 0.87 Co 0.1 Al 0.03 The coating material is tungsten oxide, with O2. The molar ratio of W to the matrix material in the coating is 0.01:1. The thickness of the coating is 1.8 nm.
[0155] The preparation method of the cathode material provided in this comparative example is basically the same as that in Example 1, except that cobalt oxide is not added in step (2).
[0156] Comparative Example 3
[0157] The cathode material provided in this comparative example includes a substrate material and a coating layer covering the surface of the substrate material. The substrate material has the chemical formula LiNi. 0.76 Co 0.1 Al 0.04 Sb 0.1 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.01:0.01:1. The thickness of the coating is 2.4 nm.
[0158] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 5, except that the molar ratio of antimony element in antimony trioxide to nickel cobalt hydroxide in step (1) is 0.1:1, that is, b = 0.1.
[0159] Comparative Example 4
[0160] The cathode material provided in this comparative example includes a substrate material and a coating layer covering the surface of the substrate material. The substrate material has the chemical formula Li. 1.045 Ni 0.7 Co 0.2 Al 0.1 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.01:0.01:1. The thickness of the coating is 2.3 μm.
[0161] The preparation method of the cathode material provided in this comparative example is basically the same as that in Example 1, the only difference being that in step (1), Ni is used... 0.9 Co 0.1 (OH)2 is replaced with Ni 0.8 Co 0.2 (OH)2, i.e., x = 0.2.
[0162] Comparative Example 5
[0163] The cathode material provided in this comparative example includes a substrate material and a coating layer covering the surface of the substrate material. The substrate material has the chemical formula Li. 1.045 Ni 0.7 Co 0.1 Al 0.2 The coating material is cobalt oxide and tungsten oxide. The molar ratio of Co in the coating, W in the coating, and the matrix material is 0.01:0.01:1. The thickness of the coating is 2.2 nm.
[0164] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 1, except that the molar ratio of aluminum element in alumina to nickel cobalt hydroxide in step (1) is 0.2:1, i.e., y = 0.2.
[0165] Comparative Example 6
[0166] The preparation method of the cathode material provided in this comparative example is basically the same as that in comparative example 5, except that the calcination in step (1) is: kept at 740℃ for 18h, during which the heating rate is 2.5℃ / min.
[0167] Comparative Example 7
[0168] The cathode material and its preparation method provided in this comparative example are basically the same as those in Comparative Example 5, except that the molar ratio of Co element in the coating layer to the matrix material is 0.1:1. The thickness of the coating layer is 5.5 nm.
[0169] Comparative Example 8
[0170] The cathode material and its preparation method provided in this comparative example are basically the same as those in Comparative Example 5, except that the molar ratio of W element to matrix material in the coating layer is 0.1:1. The thickness of the coating layer is 5.8 nm.
[0171] Comparative Example 9
[0172] The cathode material provided in this comparative example includes a substrate material and a coating layer covering the surface of the substrate material. The chemical formula of the substrate material is the same as in Example 1, and the coating layer is composed of cobalt oxide and manganese oxide. The molar ratio of Co in the coating layer, Mn in the coating layer, and the substrate material is 0.01:0.01:1. The thickness of the coating layer is the same as in Example 1.
[0173] The preparation method of the cathode material provided in this comparative example is basically the same as that in Example 1, except that tungsten oxide is replaced with manganese oxide in step (2), wherein the molar ratio of cobalt, manganese and matrix material is 0.01:0.01:1.
[0174] Comparative Example 10
[0175] The cathode material provided in this comparative example includes a substrate material and a coating layer covering the surface of the substrate material. The chemical formula of the substrate material is the same as in Example 1, and the coating layer is made of alumina and tungsten oxide. The molar ratio of Al, W, and substrate material in the coating layer is 0.01:0.01:1. The thickness of the coating layer is the same as in Example 1.
[0176] The preparation method of the cathode material provided in this comparative example is basically the same as that in Example 1, except that cobalt oxide is replaced with aluminum oxide in step (2), wherein the molar ratio of aluminum, tungsten and matrix material is 0.01:0.01:1.
[0177] Experimental Example
[0178] The positive electrode materials prepared in each embodiment and comparative example, as well as the matrix material obtained in step (1) of Example 1, were used as positive electrode active materials. The positive electrode active materials were mixed with acetylene black and PVDF at a mass ratio of 90:4:6, coated onto an aluminum foil current collector, dried at 100°C, rolled, and punched into round sheets with a diameter of 16 mm using a punching machine. The sheets were then vacuum dried at 120°C for 12 h. In an argon glove box, lithium sheets were used as negative electrodes, 1 mol / L LiPF6 EC+DMC+DEC solution was used as electrolyte, and Celgard 2400 was used as separator to make CR2032 coin cells. After standing for 8 h, electrochemical charge-discharge cycle tests were performed on a Wuhan LAND CT3001A charge-discharge tester. The voltage range was 2.5~4.25V (vs. Li + / Li), with a current of 20mA / g, initial DC internal resistance (hereinafter referred to as DCR) and 100-cycle DCR tests were performed at 100% SOC (fully charged). The results are shown in Table 1.
[0179] The test methods for initial DCR and 100-cycle DCR are as follows: a fully charged battery is left to stand for 1 hour; the battery is adjusted to 100% SOC using a 1C current; the battery is left to stand for 30 minutes, and the voltage V0 at this time is recorded as the OCV of 100% SOC; the battery is discharged using a discharge current I1 for 60 seconds, and the voltage V1 at the 60th second is recorded; the formula for calculating the DC internal resistance of discharge is: DCR=(V0-V1) / I1.
[0180] Table 1 Initial DCR and 100-cycle DCR
[0181]
[0182]
[0183] Furthermore, the cycle DCR growth rate results of each battery and the capacity retention test results of each battery after 100 cycles at 25°C and 0.5C are shown in Table 2 below.
[0184] The calculation method for the cyclic DCR growth rate ΔDCR is as follows: ΔDCR = DCR 100周 / DCR 1周 *100%, of which DCR 100周 For 100-cycle DCR, DCR 1周 This is the initial DCR.
[0185] Table 2 Cyclic DCR Growth Rate and Capacity Retention Rate
[0186]
[0187]
[0188] Among them, such as Figure 1 The figure shown is a test graph of the capacity retention rate of the cathode material provided in Example 1 after 100 cycles at 25°C and 0.5C.
[0189] As can be seen from Tables 1 and 2, compared with cobalt coating alone (Comparative Example 1) or tungsten coating alone (Comparative Example 2), cobalt-tungsten co-coating can significantly reduce the initial DCR at 100% SOC, the DCR at 100 cycles, and the growth rate of the cycle DCR, and improve the capacity retention at 100 cycles.
[0190] It is evident that the cathode material provided by this invention, through cobalt-tungsten co-coating modification, solves the problems of high initial DCR and excessively rapid DCR growth, thereby reducing the heat generation level of the battery, improving its safety performance, and alleviating capacity decay.
[0191] Experimental Example 2
[0192] The lithium-nickel mixing ratio and residual alkali content of the cathode materials prepared in each embodiment and comparative example are shown in Table 3.
[0193] The test method for lithium-nickel mixing ratio is as follows: the cathode material powder is placed in the sample stage of the XRD test instrument (model Bruker D8), and a scanning rate of 1° / min is used with a scanning angle range of 10° to 80°. The above XRD data is processed by using GSAS refinement and Pawley full spectrum fitting method to refine the XRD data to obtain the lithium-nickel mixing ratio.
[0194] The method for testing residual alkali content is as follows: Dissolve the residual alkali on the surface of 1g sample (i.e., positive electrode material) in 100mL of water, filter and take the filtrate, titrate with hydrochloric acid standard titration solution, determine the titration endpoint by the potential jump during the reaction process, calculate its content, and obtain the residual alkali content by conversion.
[0195] Table 3 Lithium-nickel mixing rate and residual alkali content
[0196] Group Lithium-nickel mixing ratio (%) Residual alkali content (ppm) Example 1 1.80 2345 Example 2 1.75 2295 Example 3 1.76 2256 Example 4 1.81 2354 Example 5 1.88 2401 Example 6 1.90 2385 Example 7 1.92 2451 Example 8 1.93 2444 Example 9 1.95 2476 Example 10 1.83 2245 Comparative Example 1 1.98 2555 Comparative Example 2 2.06 2651 Comparative Example 3 2.08 2781 Comparative Example 4 2.08 2741 Comparative Example 5 2.09 2801 Comparative Example 6 2.07 2850 Comparative Example 7 1.95 2755 Comparative Example 8 1.98 2762 Comparative Example 9 2.10 2901 Comparative Example 10 2.05 2896
[0197] As shown in Table 3, the cathode materials prepared in each embodiment have low lithium-nickel mixing rates and low residual alkali content. However, Comparative Example 2, due to the lack of cobalt coating, exhibits higher lithium-nickel mixing rates and higher residual alkali content.
[0198] Experimental Example 3
[0199] The cathode material prepared in Example 1 was subjected to SEM testing, and the results are as follows: Figure 2 As shown, this demonstrates that cobalt oxide and tungsten oxide were successfully coated on the surface of the substrate material.
[0200] Although the present invention has been illustrated and described with specific embodiments, it should be understood that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; those skilled in the art should understand that modifications can be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein, without departing from the spirit and scope of the present invention; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention; therefore, this means that all such substitutions and modifications that fall within the scope of the present invention are included in the appended claims.
Claims
1. A positive electrode material, characterized in that, The initial DC internal resistance of a battery containing the aforementioned positive electrode material is ≤10mΩ, and the rate of increase in DC internal resistance after 100 cycles is ≤143.5%. The positive electrode material includes a matrix material and a coating layer covering the surface of the matrix material; The base material has the chemical formula Li a Ni 1-x-y-b Co x Al y M b O2; wherein, 1≤a≤1.06, 0<x≤0.1, 0<y≤0.1, 0≤b≤0.05; M includes at least one of Ga, W, Zr, B, Sb, Mo, Ti, La and Sn elements; The coating layer includes Co and W elements; The thickness of the coating layer is 2~4 nm; The molar ratio of Co to W in the coating layer is 1:1.0~1.
5.
2. The cathode material according to claim 1, characterized in that, It includes at least one of the following features (1) to (4): (1) The DC internal resistance of a battery containing the positive electrode material after 100 cycles is ≤20mΩ; (2) The capacity retention rate of the battery containing the positive electrode material after 100 cycles is ≥96.5%; (3) The lithium-nickel mixing ratio of the cathode material is ≤2.0%; (4) The residual alkali content of the cathode material is ≤0.25%.
3. The cathode material according to claim 1, characterized in that, The molar ratio of Co in the coating layer to the matrix material is 0.01~0.015:1; And / or, the molar ratio of W element in the coating layer to the matrix material is 0.01~0.015:
1.
4. The method for preparing the cathode material according to any one of claims 1 to 3, characterized in that, Includes the following steps: The cathode material is obtained by sintering a mixture of a matrix material, a Co-containing coating agent, and a W-containing coating agent. The coating agent includes a Co-containing coating agent and a W-containing coating agent.
5. The method for preparing the cathode material according to claim 4, characterized in that, The sintering temperature is 500~700℃; And / or, the holding time for sintering is 5 to 7 hours.
6. The method for preparing the cathode material according to claim 4, characterized in that, The matrix material is mainly prepared by calcining a mixture of nickel cobalt hydroxide, lithium source and aluminum source. Alternatively, the matrix material is mainly prepared by calcining a mixture of nickel cobalt hydroxide, lithium source, aluminum source and dopant; wherein the doping element in the dopant includes at least one of Ga, W, Zr, B, Sb, Mo, Ti, La and Sn.
7. The method for preparing the cathode material according to claim 6, characterized in that, The calcination specifically includes: first holding at 500~700℃ for 5~7h, and then holding at 600~800℃ for 12~16h.
8. A positive electrode plate, characterized in that, Includes the cathode material as described in any one of claims 1 to 3.
9. A lithium-ion battery, characterized in that, Includes the positive electrode as described in claim 8.
10. Electrical equipment, characterized in that, Including the lithium-ion battery as described in claim 9.
Citation Information
Patent Citations
A method for preparing lithium nickel cobalt aluminate cathode material and lithium nickel cobalt aluminate prepared by the method
CN109148872A
Modified ternary positive electrode material, preparation method thereof and lithium ion battery
CN116666637A
Composite ternary positive electrode material and preparation method thereof, positive electrode plate and lithium ion battery
CN116706035A