A lithium ion battery infiltration process

The lithium-ion battery immersion process, which involves vacuuming, staged electrolyte injection, and high-temperature stirring, solves the problem of uneven immersion inside the cell, achieving uniform distribution of electrolyte within the cell and improving battery production efficiency and performance.

CN117613399BActive Publication Date: 2026-11-20MEIZHOU LIANGNENG NEW ENERGY SCI & TECHCO
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311529081.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-16
Publication Date
2026-11-20
Estimated Expiration
2043-11-16

AI Technical Summary

Technical Problem

Existing lithium-ion battery impregnation methods cannot guarantee complete impregnation of the positive and negative electrode materials and separator inside the cell, especially under high density conditions, which leads to impregnation difficulties and affects production efficiency and battery performance.

Method used

After vacuuming and replacing the drying gas, low-concentration and high-concentration electrolytes are injected in stages. Through forward and reverse rotation and high-temperature stirring, combined with high-temperature drying chamber treatment, the uniform distribution and rapid wetting of electrolyte inside the cell are ensured.

Benefits of technology

It significantly shortens the electrolyte wetting time, improves production efficiency, enhances the wetting effect, and improves the charge-discharge cycle performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117613399B_ABST
    Figure CN117613399B_ABST
Patent Text Reader

Abstract

The application discloses a kind of lithium ion battery infiltration processes, by the dry cooling of baked battery, then vacuumizing and replacement dry gas operation are carried out, then first inject low concentration electrolyte and carry out positive and negative reverse stirring, again inject high concentration electrolyte and carry out positive and negative reverse stirring, finally again the battery is moved to high-temperature drying room and continues to carry out positive and negative reverse action for a certain time, after standing, the battery is formed and activated, complete charging.The whole process step of the application is simple, and the operability is strong, can effectively shorten electrolyte infiltration time, improve production efficiency, reduce production energy consumption, greatly improve the infiltration effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery production technology, and specifically to a lithium-ion battery impregnation process. Background Technology

[0002] Electrolyte is one of the four key materials in lithium-ion batteries, often referred to as the "blood" of the battery. Its role is to conduct electrons between the positive and negative electrodes, and it is crucial for achieving the high voltage and high specific energy of lithium-ion batteries. Simultaneously, the electrolyte also acts as a lithium-ion channel, enabling reversible cyclic charging. The purpose of the electrolyte injection process in lithium-ion cells is to inject a certain amount of electrolyte into the cell through the injection port under specific dew point conditions and within a certain time frame. At this point, some of the electrolyte begins to wet the positive and negative electrode materials and the separator inside the cell. To ensure complete wetting of the cell's interior, a certain period of rest is usually required, known in the industry as the post-injection settling process. To improve the wetting effect, manufacturers generally use vacuum injection or high-pressure injection methods, followed by resting at room temperature or high temperature to allow the electrolyte to quickly wet the positive and negative electrode materials and separator inside the cell. However, during production, it is still difficult to guarantee complete wetting of the positive and negative electrode materials and separator inside the cell. Therefore, a settling period of 18-24 hours is required after injection, significantly impacting battery production capacity. As energy density increases, high electrode compaction density leads to difficulties in electrolyte injection. Smaller porosity in the electrode reduces the amount of electrolyte it can hold, and makes electrolyte movement difficult. Difficult electrode wetting can cause battery cycle failures, and even inconsistent lithium insertion / extraction capabilities at different electrode locations, leading to lithium plating in some areas and, more seriously, thermal runaway. Currently, the traditional lithium-ion wetting process involves a single high-voltage electrolyte injection, followed by high-temperature natural resting of the electrode, pre-charging, and finally, electrolyte replenishment for formation. This method didn't present wetting difficulties for older small cylindrical, pouch, and prismatic batteries, but it's less effective for modern prismatic batteries with high compaction density. Even if electrolyte is injected initially, negative-pressure pre-charging draws it out. Poor wetting during subsequent pre-charging and formation often results in unwetted areas in the center of the positive and negative electrodes. Furthermore, the use of coated separators to ensure good adhesion between the positive and negative electrodes further complicates the wetting process.

[0003] Currently, it is difficult to further improve the electrolyte wetting problem of electrodes using traditional methods, especially for batteries with multiple square winding layers, large cylindrical diameter, and high compaction density, where improving the wetting performance of electrodes is extremely challenging. Summary of the Invention

[0004] The purpose of this invention is to solve the aforementioned technical problems existing in the battery immersion methods of the prior art, and to provide an electrolyte immersion method for soft-pack lithium-ion batteries that is simple in steps, highly operable, can shorten the electrolyte immersion time, improve production efficiency, reduce production energy consumption, and improve the immersion effect.

[0005] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: Design a lithium-ion battery wetting process, including the following steps: (1) Dry and cool the baked battery cells to 45±5℃ and place them in a drying oven with a dew point of less than or equal to -35℃; (2) Vacuuming and replacing the drying gas in the dried battery cells; (3) According to the cell model, the electrolyte is injected into the cell first. A low solute concentration electrolyte A is injected into the cell. After the electrolyte is injected, the cell is rotated N1 times in both directions. The mass fraction of the solute in the low solute concentration electrolyte A is 20% to 25%. (4) Heat the high solute concentration electrolyte B to 50±5℃, inject it into the core through a pipeline, and then rotate the core in the forward and reverse direction N2 times; the mass fraction of the solute in the high solute concentration electrolyte B is 60% to 65%. (5) Move the battery cell to a high-temperature drying room and continuously rotate it in both directions for 0.5 to 1 hour. After completion, let it stand for 8 to 16 hours. (6) Activate the battery cell to complete the charging process.

[0006] In the above technical solution, step (2) can effectively extract most of the gas inside the core by vacuuming and replacing the dry gas; step (3) utilizes the high temperature maintained by the core after liquid injection, and the injection of low solute concentration electrolyte A can improve the wetting angle. At the same time, the low concentration of electrolyte results in a faster flow rate. Reversing the core can limit the resistance of the electrolyte to overcome the resistance of the particle surface and deep air and quickly enter the interior through the cavity; in step (4), heating the high concentration electrolyte can compensate for the heat loss of the core and electrolyte due to reversing stirring during the entire liquid injection process, and maintain the temperature consistency inside the core. By dividing the electrolyte into low concentration and high concentration liquid injection, there is a concentration difference between the components. The components will move from the high concentration area to the low concentration area and diffuse, which can greatly improve the wetting effect; in step (5), the core after liquid injection is rapidly stirred in both forward and reverse directions, so that the electrode liquid and nitrogen inside the core form convection, which will make the entire solution flow and form a natural convection effect.

[0007] Preferably, the vacuuming and purging process in step (2) is as follows: vacuum degree is -40kpa to -50kpa, vacuum is maintained for 25 to 35 seconds, and venting time is 4 to 8 seconds.

[0008] Preferably, in step (3), the number of forward and reverse rotations N1 of the battery cell is 2 to 3 times, the rotation speed is 20 to 25 rpm, and the time for each forward and reverse rotation is 10 to 15 seconds.

[0009] Preferably, in step (4), the number of forward and reverse rotations N2 of the battery cell is 5 to 8 times, the rotation speed is 30 to 35 rpm, and the time for each forward and reverse rotation is 20 to 30 seconds.

[0010] Preferably, in steps (3) and (4), the temperature inside the drying chamber is maintained at 15-30°C and the dew point is ≤-30°C during the liquid injection process.

[0011] Preferably, in steps (3) and (4), a high-concentration electrolyte pump is used for electrolyte injection, and the low-concentration electrolyte and the high-concentration electrolyte are respectively transported to the high-concentration electrolyte pump through the injection pipeline; the battery cell is always in the drying box during the injection process.

[0012] Preferably, the ratio of the injection volume of the low-solute-concentration electrolyte A to the high-solute-concentration electrolyte B is 1.3-1.9:1.

[0013] Preferably, the electrolyte is made of a solute, a solvent, and an additive, wherein the solvent is one or more of propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC); the solute is one or more of lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), and lithium bis(fluorosulfonyl)imide (LiFSI); and the additive is vinylene carbonate (VC) or fluoroethylene carbonate (FEC) or a mixture of both.

[0014] Preferably, in step (5), the rotation speed of the battery cell in both forward and reverse directions is 30 to 35 rpm.

[0015] Preferably, in step (5), the temperature inside the high-temperature drying chamber is maintained at 55-65°C.

[0016] The beneficial effects of this invention are as follows: By performing vacuuming and gas replacement operations on the battery cells after baking, drying and cooling, the gas inside the battery cells can be evacuated in one go, eliminating the need for multiple vacuuming and gas replacement operations and saving evacuation and gas exchange time. Utilizing the high temperature maintained by the battery cell body after electrolyte injection, the injection of low-solute-concentration electrolyte A can improve the wetting angle. At the same time, the low electrolyte concentration and fast flow rate, when the battery cell is rotated forward and backward, can restrict the electrolyte to overcome the resistance of the particle surface and deep air and quickly enter the interior through the pores.

[0017] Heating the high-concentration electrolyte can compensate for the heat loss of the core and electrolyte due to forward and reverse stirring during the entire electrolyte injection process, maintaining the temperature consistency inside the core. By injecting the electrolyte in separate low-concentration and high-concentration portions, a concentration difference is created between the components. These components will move and diffuse from areas of high concentration to areas of low concentration. The relative motion between the diffused particles and the solution itself can greatly improve the wetting effect. Rapid forward and reverse stirring of the core causes convection between the electrode liquid and nitrogen gas inside the core, which makes the entire solution flow and creates a natural convection effect, further improving the wetting effect of the battery cell.

[0018] High-concentration electrolyte injection pipelines and low-concentration electrolyte injection pipelines are used to deliver the electrolyte to the Haiba pump for injection. Multiple drying chambers can be connected simultaneously to achieve fully automated large-scale production, which is convenient to operate and highly consistent.

[0019] After electrolyte injection, the battery cell is stirred in both forward and reverse directions in a high-temperature drying chamber to maintain a constant temperature environment. This improves the temperature uniformity of each part and corner of the cell, allowing the electrolyte to fully wet every part. For cylindrical cores, especially cylindrical cores with a full tab design, this can significantly improve the wetting effect and greatly shorten the wetting time.

[0020] The overall process of this invention is simple and highly operable, which can effectively shorten the electrolyte wetting time, improve production efficiency, reduce production energy consumption, and significantly improve the wetting effect. Attached Figure Description

[0021] Figure 1 This is a schematic diagram of the injection process; Figure 2 This is a schematic diagram of the microstructure of the electrode cavity; Figure 3 The diagram shows the capacity decay of the battery cell in the invention example and the battery cell in the embodiment after 500 cycles at room temperature.

[0022] Figure 4 The diagram shows the capacity decay of the battery cell in the invention example and the battery cell in the embodiment after 400 cycles at a high temperature of 45°C. Example

[0023] The following examples illustrate specific embodiments of the present invention. However, these examples are merely for illustrative purposes and do not limit the scope of the invention in any way. Unless otherwise specified, the equipment components involved in the following examples are conventional equipment components; and unless otherwise specified, the industrial raw materials involved are commercially available conventional industrial raw materials.

[0024] Example 1: Take the same model of battery cell 906090 from the same system, inject 20g of liquid (16g solute + 3g solvent + 1g additive) for production, and number it as 6#-10#.

[0025] (1) Dry and cool the baked battery cells to 45°C and place them in a drying oven with a dew point of less than or equal to -35°C; (2) The battery cell is evacuated and replaced with dry gas. The vacuum level is -40 kPa, the vacuum is maintained for 25 seconds, and the gas is released for 4 seconds.

[0026] (3) The amount of electrolyte to be injected according to the cell model.

[0027] The electrolyte is made of solute, solvent, and additives, with the three raw materials accounting for 80%, 15%, and 5% by mass, respectively. The electrolyte is prepared into high-concentration electrolyte B (62.5% solute + 5% solvent + 2.5% additives) 11.5g and low-concentration electrolyte A (30% solute + 10% solvent + 2.5% additives) 8.5g, which are respectively transported to the Haiba pump through the high-concentration electrolyte injection pipeline and the low-concentration electrolyte injection pipeline. Then, the battery cell is scanned and weighed. First, the low-concentration electrolyte A is injected into the battery cell. After injection, the battery cell is stirred in both forward and reverse directions twice, with a rotation speed of 20 rpm and a forward and reverse rotation time of 10 seconds each time.

[0028] (4) Heat the high solute concentration electrolyte B to 50°C and inject it into the core through the pipeline; after injection, stir the core in both forward and reverse directions 5 times, with a rotation speed of 30 rpm and a forward and reverse rotation time of 20 seconds each time.

[0029] During the liquid injection process in steps (3) and (4), the temperature inside the drying chamber is maintained at 15-30℃, and the dew point is ≤-30℃.

[0030] (5) Move the battery cell to the high-temperature drying chamber, add high-temperature drying nitrogen, and keep the temperature in the high-temperature drying chamber at 55-65℃. The battery cell is mixed and stirred in both forward and reverse directions in a constant temperature environment for 0.5 to 1 hour, and then the stirring is completed and the cell is allowed to stand.

[0031] (6) Activate the battery cell to complete the charging process.

[0032] Example 2: Take the same model of battery cell 906090 from the same system, inject 20g of liquid (16g of solute + 3g of solvent + 1g of additive) for production, and number it as 11#-15#.

[0033] (1) Dry and cool the baked battery cells to 45°C and place them in a drying oven with a dew point of less than or equal to -35°C.

[0034] (2) The battery cell is evacuated and replaced with dry gas. The vacuum level is -50 kPa, the vacuum is maintained for 35 seconds, and the gas is released for 8 seconds.

[0035] (3) The amount of electrolyte to be injected according to the cell model.

[0036] The electrolyte is made of solute, solvent, and additives, with the three raw materials accounting for 80%, 15%, and 5% by mass, respectively. The electrolyte is prepared into high-concentration electrolyte B (60% solute + 2.5% solvent + 2.5% additives) 13g and low-concentration electrolyte A (20% solute + 12.5% ​​solvent + 2.5% additives) 7g, respectively, and transported to the Haiba pump through the high-concentration electrolyte injection pipeline and the low-concentration electrolyte injection pipeline, respectively. Then, the battery cell is scanned and weighed. First, the low-concentration electrolyte A is injected. After injection, the battery cell is stirred in both forward and reverse directions 3 times, with a rotation speed of 25 rpm and a forward and reverse rotation time of 15 seconds each time.

[0037] (4) Heat the high solute concentration electrolyte B to 55°C and inject it into the core through a pipeline; after injection, stir the core in both forward and reverse directions 8 times, with a rotation speed R of 35 rpm and a forward and reverse time of 30 seconds each time.

[0038] During the liquid injection process in steps (3) and (4), the temperature inside the drying chamber is maintained at 15-30℃, and the dew point is ≤-30℃.

[0039] (5) Move the battery cell to the high-temperature drying chamber, add high-temperature drying nitrogen, and keep the temperature in the high-temperature drying chamber at 55-65℃. The battery cell is mixed and stirred in both forward and reverse directions in a constant temperature environment at a speed of 25 rpm for 1 hour, and then the stirring is completed and the cell is allowed to stand.

[0040] (6) Activate the battery cell to complete the charging process.

[0041] Traditional example: Take the same model of battery cell 906090 from the same system, use the traditional liquid injection method, inject 20g of liquid at one time (16g of solute + 3g of solvent + 1g of additive) for production, and number it 1#-5#.

[0042] The batteries prepared according to the embodiments of the present invention and the conventional examples were subjected to a 300-cycle charge-discharge capacity retention test. The test results are shown in the table below.

[0043]

[0044] Appendix Figure 3 Capacity decay graphs of conventional and exemplary battery cells after 500 cycles at room temperature are shown; (See attached graph) Figure 4 The table shows the capacity decay of conventional and example battery cells after 400 cycles at 45°C. The results are presented in the table above and in the attached diagram. Figure 3 Appendix Figure 4 It can be seen that the battery prepared by the lithium-ion battery impregnation process of the present invention has a significantly higher capacity retention rate after 300 charge-discharge cycles than the battery prepared by the traditional one-time liquid injection process; the capacity decay effect of the cell in the embodiment of the present invention after 500 cycles at room temperature and 400 cycles at 45°C is better than that of the cell in the traditional example.

[0045] The present invention has been described in detail above with reference to the embodiments. However, those skilled in the art will understand that, without departing from the spirit of the present invention, various specific parameters in the above embodiments can be changed to form multiple specific embodiments, all of which are common variations of the present invention, and will not be described in detail here.

Claims

1. A lithium-ion battery impregnation process, characterized in that, Includes the following steps: (1) Dry and cool the baked battery cells to 45±5℃ and place them in a drying oven with a dew point of less than or equal to -35℃; (2) Vacuuming and replacing the drying gas in the dried battery cells; (3) According to the cell model, the electrolyte is injected into the cell first. A low solute concentration electrolyte A is injected into the cell. After the electrolyte is injected, the cell is rotated N1 times in both directions. The mass fraction of the solute in the low solute concentration electrolyte A is 20% to 25%. (4) Heat the high solute concentration electrolyte B to 50±5℃, inject it into the core through a pipeline, and then rotate the core in the forward and reverse direction N2 times; the mass fraction of the solute in the high solute concentration electrolyte B is 60% to 65%. (5) Move the battery cell to a high-temperature drying room and continuously rotate it in both directions for 0.5 to 1 hour. After completion, let it stand for 8 to 16 hours. (6) Activate the battery cell to complete the charging process.

2. The lithium-ion battery impregnation process according to claim 1, characterized in that, The vacuuming and purging process in step (2) is as follows: the vacuum is -40 kPa to -50 kPa, the vacuum is maintained for 25 to 35 seconds, and the venting time is 4 to 8 seconds.

3. The lithium-ion battery impregnation process according to claim 1, characterized in that, In step (3), the number of forward and reverse rotations N1 of the battery cell is 2 to 3 times, the rotation speed is 20 to 25 rpm, and the time for each forward and reverse rotation is 10 to 15 seconds.

4. The lithium-ion battery impregnation process according to claim 1, characterized in that, In step (4), the number of forward and reverse rotations N2 of the battery cell is 5 to 8 times, the rotation speed is 30 to 35 rpm, and the time for each forward and reverse rotation is 20 to 30 seconds.

5. The lithium-ion battery impregnation process according to claim 1, characterized in that, In steps (3) and (4), the temperature inside the drying chamber is maintained at 15-30℃ and the dew point is ≤-30℃ during the liquid injection process.

6. The lithium-ion battery impregnation process according to claim 1, characterized in that, In steps (3) and (4), a high-concentration electrolyte pump is used for electrolyte injection. The low-concentration electrolyte and the high-concentration electrolyte are respectively transported to the high-concentration electrolyte pump through the injection pipeline. During the electrolyte injection process, the battery cell is always in the drying chamber.

7. The lithium-ion battery impregnation process according to claim 1, characterized in that, The ratio of the injection volume of the low-solute-concentration electrolyte A to the high-solute-concentration electrolyte B is 1.3-1.9:

1.

8. The lithium-ion battery impregnation process according to claim 1, characterized in that, The electrolyte is made of a solute, a solvent, and additives. The solvent is one or more of propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, and methyl ethyl carbonate. The solute is one or more of lithium tetrafluoroborate, lithium hexafluorophosphate, or lithium bis(fluorosulfonyl)imide. The additives are vinylene carbonate, fluoroethylene carbonate, or a mixture of both.

9. The lithium-ion battery impregnation process according to claim 1, characterized in that, In step (5), the rotation speed of the battery cell in both directions is 30 to 35 rpm.

10. The lithium-ion battery impregnation process according to claim 1, characterized in that, In step (5), the temperature inside the high-temperature drying chamber is maintained at 55-65℃.

Citation Information

Patent Citations

  • Battery device and manufacturing method of the same

    JP2015103284A

  • Non-aqueous electrolyte-type lithium ion secondary cell and manufacturing method thereof, and a vehicle or device in which non-aqueous electrolyte-type lithium ion secondary cells are mounted

    WO2010125642A1