A laser weaving wire welding method

By employing a narrow-gap laser oscillating filler wire welding method, the problem of difficult weld formation control in the welding of thick plates with large blunt edge bevels has been solved, achieving efficient and high-quality welding of thick plates and ensuring welding quality and speed.

CN117620417BActive Publication Date: 2026-11-24GW (SHANGHAI) LASER TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311860877.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2023-08-23
Filing Date
2023-12-31
Publication Date
2026-11-24
Estimated Expiration
2043-12-31

AI Technical Summary

Technical Problem

In existing laser welding of thick plates with large blunt edge bevels, weld formation is difficult to control, and problems such as weld back hump, nodules, lack of fusion, and wire wobbling are prone to occur, affecting welding efficiency and quality.

Method used

A narrow-gap laser oscillating filler wire welding method is adopted. By reasonably setting the blunt edge size, bevel angle and laser power, and combining the beam oscillation with filler wire welding, the laser spot and the welding wire are made to coincide. The oscillation amplitude and frequency are optimized through iterative calculation to ensure welding quality.

Benefits of technology

It achieves stability and efficiency in laser welding of thick plates with large blunt edges and narrow gaps, prevents incomplete fusion and penetration, ensures high-quality weld formation, and improves welding speed and heat input stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117620417B_ABST
    Figure CN117620417B_ABST
Patent Text Reader

Abstract

This invention discloses a laser oscillating filler wire welding method, which can solve the problem of incomplete fusion in narrow gap laser filler wire welding. Through iterative calculation, the oscillation amplitude is increased to achieve the width of the upper edge of the cross section of the filler wire for each bevel. Multi-layer and multi-pass automatic welding can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a laser oscillating wire welding method, and more particularly to a narrow-gap laser oscillating wire welding method. Background Technology

[0002] With the development of laser welding technology, high-end equipment manufacturing industries such as energy equipment, shipbuilding, petrochemicals, and marine engineering have an urgent need for efficient and high-quality welding of medium and thick plates in large structural components. There are many existing welding methods for thick plates, among which the narrow-gap laser wire-filled welding method for thick plates is a highly efficient and high-quality welding technology. Compared with traditional arc welding technology, it has advantages such as faster welding speed, lower heat input, higher joint strength, and finer weld grains. When welding thick and very thick plates using this method, the filler area of ​​the bevel should generally be minimized. This necessitates a large blunt edge and narrow bevel design. However, existing high-power laser welding with large blunt edge bevels easily results in the formation of a liquid column at the molten pool front, generating significant spatter and severely impacting the formation of the laser-cut root pass weld. Furthermore, in the fill pass weld, a large wire feed is required to maximize deposition efficiency. However, due to the narrow bevel width, a large wire feed results in a large depth-to-width ratio (i.e., a small weld formation coefficient) in a single weld layer. During weld solidification, the weld center is prone to solidification last, and due to the lack of liquid metal compensation, crystallization cracks eventually form at the weld center. Therefore, in actual welding, it is difficult to use a large wire feed to control the weld formation coefficient, which severely affects welding efficiency. Therefore, to solve the above technical problems, it is essential to provide a highly efficient method for welding medium and thick plates using a large blunt edge and narrow gap oscillating beam laser.

[0003] Currently, the pressing problems to be solved in the welding of thick plates with large blunt edge bevels include: During the root pass, when welding 30mm or even thicker steel plates (such as thick 304 stainless steel plates) in a single laser pass, the difficulty of single-laser welding of thick plates is very high. Often, humps, nodules, or incomplete penetration appear on the back of the weld, and the weld on the front is not smooth, thus affecting the filler wire process. Furthermore, during the gap filling process, incomplete fusion easily occurs on the sidewalls, and the welding wire near the molten pool wobbles, causing the laser to fail to melt the welding wire. Summary of the Invention

[0004] To address the shortcomings of existing technologies, this invention provides a narrow-gap laser oscillating filler wire welding method, which overcomes the deficiencies of existing technologies and is rationally designed.

[0005] To achieve the above objectives, the present invention provides the following technical solution:

[0006] This invention provides a laser oscillating filler wire welding method.

[0007] A laser oscillating filler wire welding method, characterized by comprising the following steps:

[0008] S1: Prepare a steel plate to be welded with a thickness greater than 30 mm; S2: Set a groove, when the thickness of the steel plate is H, the size of the selected blunt edge is L, which needs to satisfy L>H / 2-(H-22mm) / 4, L<H / 2+(H-22mm) / 4 and L<36mm, where H ranges from 30 mm to 100 mm; the width of the bottom edge of the cross section of the groove is 1 mm-5 mm, and the groove surface angle α is less than 5 degrees; S3: Use laser for backing welding, the output power of the backing laser needs to be greater than 15 kW and less than 30 kW; S4: Perform wire filling welding, which is multiple passes of wire filling welding from the bottom of the groove to the upper side, and the beam is oscillated during laser welding.

[0009] Preferably, the width of the lower side of the cross section of the groove after each wire filling welding is the beam oscillation amplitude during the current wire filling welding.

[0010] Preferably, as the wire filling process proceeds, since the lateral dimension of the lower side of the groove cross section becomes larger and larger, the oscillation amplitude needs to be adjusted, and the oscillation frequency is reduced while increasing the oscillation amplitude so that the energy density remains unchanged.

[0011] Preferably, single-side groove welding is adopted, the groove is a J-shaped or U-shaped groove, and the welding speed is 20-35 mm / s.

[0012] Preferably, the width of the bottom surface of the groove is d1, the angle of the groove surface is α, and in the multi-layer wire filling welding from the bottom to the top, after the first layer of welding is completed, the cross-sectional width of the groove becomes d2, that is, during the first wire filling welding, the oscillation amplitude is set to d2, after the second layer of welding is completed, the cross-sectional width of the groove becomes d3, that is, during the second wire filling welding, the oscillation amplitude is set to d3, and so on, after the Nth layer of welding is completed, the cross-sectional width of the groove becomes d N+1 , that is, during the Nth wire filling welding, the oscillation amplitude is set to d N+1 .

[0013] Preferably, the cross-sectional shape of the groove of the steel plate is trapezoidal.

[0014] Preferably, the system of equations for iterative calculation includes the following formulas:

[0015] s1=(d1+d2)h1 / 2 Formula (1)

[0016] h1=(d2-d1) / (2tanα) Formula (2)

[0017]

[0018] Where d1 is the width of the bottom of the bevel; d2 is the first swing amplitude; h1 is the first filling depth; α is the angle of one side of the bevel; V1 is the volume of the gap requiring the first filling; s1 is the cross-sectional size of the gap requiring the first filling; v w v is the welding speed. f Here, d0 is the wire feeding speed, t is the wire diameter, and t is the single welding time. The filler wire welding process includes the following steps: a) First filler wire welding: Solve the bevel section width d2 after the first filler wire by solving equations (1), (2), and (3), and then set the swing amplitude as d2; b) Second filler wire welding: Use the result of the first welding as a basis for iterative calculation, solve the bevel section width d3 after the second filler wire by iteratively solving equations (1), (2), and (3), and then set the swing amplitude as d3; c) Third filler wire welding: Use the result of the second welding as a basis for iterative calculation, solve the bevel section width d3 after the second filler wire by iteratively solving equations (1), (2), and (3), and then set the swing amplitude as d3; The bevel section width d4 after the third filler wire welding is solved iteratively by solving equations (1), (2), and (3) simultaneously, and then the swing amplitude is set to d4; d, the fourth filler wire welding is performed using the result of the third welding as the basis for iterative calculation. The bevel section width d5 ​​after the fourth filler wire welding is solved iteratively by solving equations (1), (2), and (3) simultaneously, and then the swing amplitude is set to d5; e, and so on, for the Nth filler wire welding, the bevel section width d after the (N-1)th welding is solved iteratively by solving equations (1), (2), and (3) simultaneously. N+1 Then set the swing amplitude to d. N+1 f. Repeat step e until the filler wire welding is complete.

[0019] Preferably, the larger the swing amplitude, the smaller the set swing frequency.

[0020] Preferably, after each filler wire welding operation, the welding head needs to be raised to a corresponding height h. N h N The value is also obtained by iterative calculation from the simultaneous equations (1), (2), and (3).

[0021] Preferably, the formula for calculating the oscillation frequency is as follows: (1-A)·d=v w / f; overlap rate A = x / d = (dL) / d; where L = v w / f, d is the swing amplitude, d is 1mm-5mm, the overlap rate A is 50%-90%; L is the center-to-center distance, the swing shape is circular; x is the width of the overlapping part; f is the swing frequency.

[0022] The beneficial effects of this invention are:

[0023] 1. This invention provides a narrow-gap laser oscillating filler wire welding method, which achieves laser spot and welding wire overlap by laser oscillation, and realizes single-laser one-time welding of steel plates 30mm or even thicker through large blunt edge narrow bevel welding.

[0024] 2. This invention rationally sets the power of laser rooting and selectively chooses the optimal range of blunt edge size, bottom width of bevel section, and bevel angle to prevent poor rooting and the inability of filler wire welding to achieve sidewall fusion. It also discovers an empirical formula for rationally selecting the range of blunt edge size so that laser rooting can achieve good rooting while avoiding incomplete fusion and preventing incomplete penetration.

[0025] 3. This invention rationally designs the welding process. At the same time, during filler wire welding, by solving for the gap and making the oscillation amplitude equal to the gap, the laser oscillation and the gap of the filler wire are perfectly matched, achieving perfect filler wire welding. By calculating the height of the filler wire using existing data during each welding and making the welding head rise to the same height, the laser focusing position is reasonable. By increasing the power and / or decreasing the oscillation frequency during each welding, the energy density during laser welding is stabilized, resulting in better welding results.

[0026] 4. Calculate a reasonable oscillation frequency using a formula to keep the energy density constant, thus making the welding more stable.

[0027] 5. A reasonable empirical formula for laser priming power can achieve sufficient priming without soldering through. Attached Figure Description

[0028] To more clearly illustrate the technical solutions in this invention or the prior art, the accompanying drawings used in the description of the prior art will be briefly introduced below.

[0029] Figure 1 This is the front side of the 40mm stainless steel weld of the present invention;

[0030] Figure 2 This is the wire feeding process for the weld seam in this invention;

[0031] Figure 3 This is the back side of the weld in this invention;

[0032] Figure 4 This is a schematic diagram of the laser oscillation characteristics;

[0033] Figure 5 This is a schematic diagram of the overlap rate of the laser oscillation;

[0034] Figure 6 This is a schematic diagram of the trapezoidal cross-section of the bevel of the present invention;

[0035] Figure 7is a schematic diagram of the width of the lower side of a groove cross-section after each wire filling welding according to the present invention. Detailed Description of the Embodiments

[0036] To make the objectives, technical solutions, and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the present invention.

[0037] The embodiment of the present invention provides a narrow-gap laser oscillating wire filling welding method, which is used for welding thick plates, such as steel plates with a thickness of 30mm-100mm. Preferably, the thickness of the steel plate is greater than 35mm, such as a steel plate with a thickness of 45mm-69mm, or even a steel plate with a thickness greater than 70mm. It adopts large blunt edge groove welding, preferably large blunt edge narrow groove welding.

[0038] Specifically, in order to form a thick steel plate by one-time welding, the present invention preferably adopts large blunt edge groove welding. For example, when the thickness of the steel plate is selected to be more than 30mm, the size of the selected blunt edge is L. Through simulation calculation, the inventor found that the size of L needs to be more than 15mm. The inventor has found an empirical formula for selecting the range of the blunt edge size when achieving good laser backing welding through long-term research. Assuming that the thickness of the steel plate is H, in single-side groove welding, it is necessary to satisfy L>H / 2-(H-22mm) / 4 to achieve a good backing ratio. At the same time, in order to avoid incomplete fusion, preferably, it is necessary to satisfy L<H / 2+(H-22mm) / 4, and also satisfy L<36mm to prevent incomplete penetration. The range of H is 30mm-100mm, preferably, the range of H is 45mm-69mm. Preferably, in order to prevent the excessive requirement for backing laser caused by the excessively thick blunt edge and according to the material properties of steel, it does not require an excessively thick blunt edge. Then usually, with the increase of H, the change of L can be slightly slower, and in some cases, L is usually preferably 15mm-25mm.

[0039] Typically, preferably, the width of the bottom edge of the bevel cross-section (the transverse width of the bevel bottom surface) d1 is 0-5mm; if d1 is too narrow, it will be detrimental to the preceding filler wire welding. To make the first filler wire welding smoother, preferably, the width of the bottom edge of the bevel cross-section d1 is greater than 1mm. To appropriately reduce the amount of filler wire used in the bevel welding and to make the filler wire welding more reliable, preferably, d1 is less than 3.5mm; preferably, the width of the bottom edge of the bevel cross-section d1 is 1.5mm-3mm. Preferably, the bevel angle 2α corresponding to the narrow bevel should be less than 12 degrees, preferably, 2α is less than 10 degrees, preferably, 2α is less than 8 degrees. The width of the bottom edge of the bevel cross-section d1 and the bevel angle α together constitute the essential meaning of the narrow gap of the present invention, thereby enabling the narrow gap filler wire welding of thick plates with large blunt edges. That is, correspondingly, preferably, the bevel angle α≤6 degrees, preferably, α≤5 degrees, preferably, α≤4 degrees, which corresponds to typical narrow gap bevel welding. In addition, in order to prevent insufficient filler wire at the bottom of the bevel, preferably, the bevel face angle α ≥ 2 degrees, preferably, the bevel face angle α ≥ 3 degrees. Based on years of experience in filler wire welding, the inventors have concluded that when 3 degrees ≤ α ≤ 4 degrees, the large blunt edge and narrow gap filler wire welding can achieve sufficient bottom filler wire and good side fusion at the same time compared to other bevel face angles.

[0040] In addition, since the thickness of the blunt edge of the base layer is relatively large, the inventors realized that the power of the laser must meet certain requirements to achieve fusion. Preferably, the output power of the base laser needs to be greater than 15KW and less than 35KW. More preferably, the output power of the base laser is greater than 20KW and less than 30KW.

[0041] The inventors realized that the ideal laser power required for priming varies depending on the thickness of the blunt edge. Through simulation and actual laser priming experiments, the inventors finally obtained an empirical formula and selected a laser priming power of P = [(L / 2mm) + 8] * KW to achieve sufficient priming without soldering through.

[0042] For example, when using a 25KW laser for the root pass, single-laser welding is employed for steel plates with a blunt edge of 15-25mm. Appropriate process parameters are controlled (welding speed 20-35mm / s, focal point at 1 / 3 of the blunt edge thickness (distance from the top surface, e.g., -5mm for a 15mm stainless steel blunt edge), and a protective gas is added to the back of the steel plate at a pressure of 0.1-0.2MPa). This invention utilizes a high-power laser with a thick blunt edge, unlike previous patents which typically had a 3-4mm thickness. This invention typically uses a 15-25mm blunt edge, fully utilizing the high-power laser for welding thicker plates, improving efficiency, and enabling the welding of even thicker plates. Because narrow-gap welding involves two processes—root pass and filler wire—when the blunt edge is thick, narrow-gap filler wire welding can weld even thicker plates with less filler wire required. Simultaneously, deformation is minimal. Since single-laser root pass is highly efficient (20-35mm / s), filler wire is not needed, resulting in lower heat input than any other thick plate welding process.

[0043] When welding with a large blunt edge bevel, filler wire is required after the root pass. To make the weld stronger, we use V-shaped, J-shaped, or U-shaped bevels when welding on one side, preferably U-shaped or V-shaped bevels.

[0044] Preferably, the cross-sectional shape of the bevel on the steel plate is trapezoidal. The width of the base of the trapezoidal cross-section of the bevel is d1 (when d1 equals 0, it is a triangular / V-shaped cross-section), and the bevel angle is α. As the filler wire process proceeds, the lateral width of the lower side of the bevel cross-section increases. Therefore, we need to control the filler wire process appropriately to ensure the accuracy of the filler wire and the strength of the weld.

[0045] The inventors realized that the laser spot and the welding wire need to coincide, and the spot size needs to be slightly larger than the welding wire size in order to completely melt the welding wire. In order to achieve perfect fusion of the two side walls, it is necessary to increase the beam oscillation. At the same time, the oscillation amplitude of the present invention is larger than that of laser filler welding technology, so as to melt the side walls and solve the problem of incomplete fusion. Since the laser spot and the welding wire need to coincide, the gap needs to be filled by oscillating filler wire. Preferably, the oscillation filler wire and the laser oscillation are basically synchronized.

[0046] Therefore, preferably, in filler wire welding: a) First, it is necessary to add a beam oscillation function, that is, the laser welding head needs to oscillate the beam; b) As the filler wire process proceeds, since the lateral dimension of the bottom edge of the bevel section becomes larger and larger (that is, the filler wire gap becomes larger and larger), it is necessary to adjust the oscillation amplitude so that the width of the bottom edge of the bevel section after each filler wire is the beam oscillation amplitude during the current filler wire. At the same time, it is necessary to increase the laser power or decrease the oscillation frequency so that the energy density per unit time remains basically unchanged (since filler wire welding is done by filling each layer of multiple layers from bottom to top, each layer of filler wire welding is considered as one filler wire welding, that is, the filler wire welding of the first layer is the first filler wire welding).

[0047] Let the lateral width of the bevel bottom be d1. In a multi-layer filler wire welding process from bottom to top, after the first layer is welded, the width of the lower side of the bevel cross-section becomes d2 (i.e., the amplitude is set to d2 during the first filler wire welding). After the second layer is welded, the width of the lower side of the bevel cross-section becomes d3 (i.e., the amplitude is set to d3 during the second filler wire welding), and so on. After the Nth layer is welded, the width of the lower side of the bevel cross-section becomes d1. N+1 (That is, during the Nth wire filler welding, the swing amplitude is set to d) N+1 ).

[0048] How to determine the beam oscillation amplitude for each welding operation, i.e., how to determine d2, d3...d N+1 It can be based on the wire feeding speed v f and welding speed v w The bevel shape parameters (d1 and α) are calculated. By calculating the volume V of each filler wire, the cross-section after each filler wire is calculated. First, the first filler wire depth h1 and the lower side width d2 of the bevel cross-section after the first filler wire are calculated (let the beam swing of the first filler wire be set as d2). Then, the second filler wire depth h2 and the lower side width d3 of the bevel cross-section after the second filler wire are calculated in the same way. Then, the Nth filler wire depth h is calculated in the same way. N The width d of the lower side of the bevel section after the Nth filling wire. N+1 .

[0049] The calculation process is as follows, for the first filler wire welding:

[0050] Formula for the cross-sectional area of ​​the fill: s1=(d1+d2)h1 / 2 Equation (1)

[0051] Using the geometric relationships of right triangles, we can obtain: h1=(d2-d1) / (2tana) Equation (2)

[0052] The gap volume is equal to the wire feeding volume:

[0053] (3)

[0054] Wherein, d1 is the width of the bottom of the bevel, generally 1-3mm; d2 is the first swing amplitude, which is also the width of the bottom edge of the bevel after the first filler wire; h1 is the first filler wire depth, generally 5mm-8mm (related to welding speed, wire feed speed and bevel size, and needs to be calculated); α is the bevel angle (i.e., bevel face angle), generally 3-4°; V1 is the volume of the gap requiring the first filler wire, and s1 is the cross-sectional size of the gap requiring the first filler wire; v w v is the welding speed. f d is the wire feed speed, d0 is the wire diameter, and t is the welding time per pass.

[0055] By combining the above three equations, namely equations (1), (2), and (3), we can solve for d2, h1, and s1 of the first filler wire welding. If we need to solve for the swing width, filler depth, etc., corresponding to the second filler wire welding, we can use the result of the first filler wire welding as a basis and calculate it using the iterative equation system composed of equations (1), (2), and (3). Similarly, by using the result of the previous filler wire welding as a basis and iteratively calculating it using equations (1), (2), and (3), we can calculate the swing width, filler depth, etc., corresponding to the current filler wire welding. Here, using the result of the previous welding as a basis means using the d obtained after the (N-1)th welding as a basis. N Substitute d1 into equations (1), (2), and (3).

[0056] That is, after the first filler wire welding is completed, the calculation of subsequent filler wire welding is an iteration of the above formula. The specific iterative formula can be expected based on mathematical common sense, as follows: the iterative formula (1) for the Nth filler wire welding becomes s. N =(d N +d N+1 )·h N / 2, the Nth filler wire welding equation (2) iteratively becomes h N =(d N+1 -d N Equation (3) is ) / (2tanα); For example, when the selected welding wire diameter d0 = 1.6 mm, the bevel size is set to d1 = 2 mm, α = 3°, and the wire feed speed is v... f The welding speed is 6 m / min, v w When the speed is 5 mm / s, v f / v w =20. By combining equations (1), (2), and (3), we can solve for d2, h1, and s1. Similarly, we can solve for d3, d4, ... d n .

[0057] By repeating this iterative process, the amplitude of each swing and the height the welding head is raised during each wire feeding can be calculated. (Preferably, other parameters remain constant, such as welding speed, wire feed speed, and defocusing amount.) The defocusing amount is the height from the laser focus to the weld seam. A focus above the weld seam indicates positive defocusing, and a focus below the weld seam indicates negative defocusing. Therefore, after each welding operation, the welding head needs to be raised by h (corresponding to h1, h2, h3...h after each wire feeding welding). N ).

[0058] Preferred embodiment 1:

[0059] Step 1: Select a 20kW laser, a wobbling welding head with collimation / focus of 100 / 250, select 40mm thick stainless steel, and open a bevel with a trapezoidal cross-section. Preferably, the dimensions are 16mm for the blunt edge, d1 = 2.5mm, and α = 3°.

[0060] Step 2: Adjust the height of the welding head so that the defocusing amount is -5mm (the focal point is located 5mm below the upper edge of the blunt edge);

[0061] Step 3: Base pass: Pass 0.1MPaAr through the bottom of the plate. After 15 seconds, set the laser power to 16000W and the welding speed to 35mm / s and perform welding. After welding, scrape off the slag on the weld surface and then blow away the slag with a high-pressure air gun.

[0062] Step 4: First filler wire welding: Solve the bevel section width d2 after the first filler wire by solving equations (1), (2), and (3), and then set the swing amplitude to d2; swing frequency = 50Hz, wire feeding speed 4m / min, welding wire at 60° with plate, and welding speed 6mm / s (the first filler wire depth h1 can be solved at the same time).

[0063] Step 5: Second filler wire welding. Using the result of the first filler wire welding as a basis, the bevel section width d3 after the second filler wire welding is solved iteratively by solving equations (1), (2), and (3). Then, the swing amplitude is set to d3; the swing frequency is 40Hz, the wire feeding speed is 4m / min, the welding wire is at 60° with the plate, and the welding speed is 6mm / s (the second filler wire depth h2 can be solved at the same time).

[0064] Step 6: Third filler wire welding. Using the result of the second filler wire welding as a basis, the bevel section width d4 after the third filler wire welding is solved iteratively by solving the simultaneous equations (1), (2), and (3). Then, the swing amplitude is set to d4; the swing frequency is 30Hz, the wire feeding speed is 4m / min, the welding wire is at 60° with the plate, and the welding speed is 6mm / s (the filler wire depth h3 of the third filler wire welding can be solved at the same time).

[0065] Step 7: Fourth filler wire welding. Using the result of the third filler wire welding as a basis, the bevel section width d5 ​​after the fourth filler wire welding is solved iteratively by solving equations (1), (2), and (3). Then, the swing amplitude is set to d5; the swing frequency is 25Hz (the larger the swing amplitude, the smaller the set swing frequency), the wire feeding speed is 4m / min, the welding wire is at 60° with the plate, and the welding speed is 6mm / s (the filler wire depth h4 of the fourth filler wire welding can be solved at the same time).

[0066] Step 8: By iterative calculation, using the result of the (N-1)th filler wire welding as a basis, for the Nth filler wire welding, the bevel width d after the next Nth filler wire welding is solved iteratively by solving equations (1), (2), and (3). N+1 Then set the swing amplitude to d. N+1 Set the corresponding oscillation frequency, wire feed speed, angle between the welding wire and the plate, welding speed, etc. (the filler depth h for the Nth time can be solved simultaneously). N ).

[0067] Step Nine: Repeat Step Eight until the filler wire welding is complete. (After each filler wire welding operation, the weld head needs to be raised to the corresponding height h.) N h N The value is also obtained by iterative calculation from the simultaneous equations (1), (2), and (3).

[0068] Example 2:

[0069] Step 1: Select a 20kW laser, a wobbling welding head with collimation / focus of 100 / 250, select 50mm thick stainless steel, and open a bevel with a trapezoidal cross-section, setting the dimensions as follows: blunt edge 20mm, h1=2.5mm, α=3°;

[0070] Step 2: Adjust the height of the welding head so that the defocusing amount is -7mm (the focal point is located 7mm below the upper edge of the blunt edge);

[0071] Step 3: Base pass: Pass 0.1MPaAr through the bottom of the plate. After 15 seconds, set the laser power to 18000W and the welding speed to 30mm / s and perform welding. After welding, scrape off the slag on the weld surface and then blow away the slag with a high-pressure air gun.

[0072] Step 4: First filler wire welding: Solve the bevel section width d3 after the first filler wire by solving equations (1), (2), and (3), and then set the swing amplitude to d3; swing frequency = 50Hz, wire feeding speed 4m / min, welding wire at 60° with plate, and welding speed 6mm / s (the first filler wire depth h1 can be solved at the same time).

[0073] Step 5: Second filler wire welding. Using the result of the first filler wire welding as a basis, the bevel section width d3 after the second filler wire welding is solved iteratively by solving equations (1), (2), and (3). Then, the swing amplitude is set to d3; the swing frequency is 40Hz, the wire feeding speed is 4m / min, the welding wire is at 60° with the plate, and the welding speed is 6mm / s (the second filler wire depth h2 can be solved at the same time).

[0074] Step 6: Third filler wire welding. Using the result of the second filler wire welding as a basis, the bevel section width d4 after the third filler wire welding is solved iteratively by solving the simultaneous equations (1), (2), and (3). Then, the swing amplitude is set to d4; the swing frequency is 30Hz, the wire feeding speed is 4m / min, the welding wire is at 60° with the plate, and the welding speed is 6mm / s (the filler wire depth h3 of the third filler wire welding can be solved at the same time).

[0075] Step 7: Fourth filler wire welding. Using the result of the third filler wire welding as a basis, the bevel section width d5 ​​after the fourth filler wire welding is solved iteratively by solving equations (1), (2), and (3). Then, the swing amplitude is set to d5; the swing frequency is 25Hz (the larger the swing amplitude, the smaller the set swing frequency), the wire feeding speed is 4m / min, the welding wire is at 60° with the plate, and the welding speed is 6mm / s (the filler wire depth h4 of the fourth filler wire welding can be solved at the same time).

[0076] Step 8: By iterative calculation, for the Nth filler wire welding, using the result of the (N-1)th filler wire welding as a basis, the bevel width d after the next Nth filler wire welding is solved iteratively by solving the simultaneous equations (1), (2), and (3). N+1 Then set the swing amplitude to d. N+1 Set the corresponding oscillation frequency (the larger the oscillation amplitude, the smaller the set oscillation frequency), wire feed speed, angle between the welding wire and the plate, welding speed, etc. (the wire filling depth h for the Nth time can be solved simultaneously). N ).

[0077] Step Nine: Repeat Step Eight until the filler wire welding is complete. (After each filler wire welding operation, the weld head needs to be raised to the corresponding height h.) N h N The value is also calculated from the simultaneous equations (1), (2), and (3).

[0078] This can solve the problem of incomplete fusion in narrow-gap laser filler wire welding. Through iterative calculation, the swing amplitude can be increased (to reach the width of the upper edge of the cross-section of each filler wire in the bevel). Multi-layer, multi-pass automatic welding can be achieved because the height of the weld head can be calculated iteratively for each filler wire. It is expected that single-sided welding can achieve a root pass of 25mm + filler wire of 35mm, and a single-sided welding of a plate thickness of 25mm + 35mm = 60mm.

[0079] Preferably, the power of each filler wire welding is generally 5KW to 10KW, and more preferably, the power of each filler wire welding is 6KW-8KW.

[0080] Furthermore, during the next filler wire welding operation after each welding cycle, the inventors realized that maintaining consistent energy density per unit area per unit time required either increasing the laser power or decreasing the oscillation frequency. The inventors also recognized that increasing the power could cause variations in burr size; therefore, to ensure consistent welding results, decreasing the oscillation frequency was preferable to achieve consistent energy density per unit time.

[0081] To maintain a consistent energy density per unit time during each wire feeding weld, the inventors realized that this could be achieved through the oscillation characteristics of the laser.

[0082] Laser oscillation characteristics such as Figure 4 The calculation of its overlap rate is as follows: Figure 5 , can be obtained

[0083] Overlap rate A = x / d = (dL) / d Equation (4)

[0084] At the same time, L = v w / f Formula (5)

[0085] Combining equations (4) and (5),

[0086] The relationship between amplitude and oscillation frequency can be obtained as follows:

[0087] We can obtain (1-A)·d=v w / f Formula (6)

[0088] The oscillation frequency for each filler wire welding can be calculated based on the oscillation amplitude to ensure stable energy density. Here, d is the oscillation amplitude, typically 1-5 mm, with an overlap rate of 50%-90%; L is the center-to-center distance (the oscillation shape is circular); x is the width of the overlapping portion; and f is the oscillation frequency, typically 20-300 Hz.

[0089] Preferably, the welding equipment includes modules such as a controller, a computing unit, a detector, and a drive unit to implement the above-mentioned automatic welding method.

[0090] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A laser-assisted oscillating filler wire welding method, characterized in that, comprising the following steps: S1: preparing a steel plate to be welded with a thickness greater than 30 mm; S2: forming a groove, wherein when the thickness of the steel plate is H, the size of the selected root face is L, which needs to satisfy L>H / 2-(H-22mm) / 4, L<H / 2+(H-22mm) / 4, and L<36mm, where H ranges from 30 mm to 100 mm; the width of the bottom edge of the cross-section of the groove is 1 mm to 5 mm, and the angle α of the groove face is less than 5 degrees; S3: performing backing welding using a laser, wherein the output power of the backing laser needs to be greater than 15 kW and less than 30 kW; S4: performing wire filling welding, which is multiple passes of wire filling welding from the bottom of the groove to the upper side, and beam oscillation is performed during laser welding; the width of the lower side edge of the groove cross-section after each wire filling welding is the beam oscillation amplitude during the current wire filling welding; the cross-sectional shape of the groove of the steel plate is trapezoidal; the iterative calculation equation set includes the following formula: Equation (1) Equation (2) Equation (3) Where d1 is the width of the bottom of the bevel; d2 is the first swing amplitude; h1 is the first filling depth; α is the angle of one side of the bevel; V1 is the volume of the gap requiring the first filling; s1 is the cross-sectional size of the gap requiring the first filling; v w v is the welding speed. f d is the wire feeding speed, d0 is the wire diameter, and t is the single welding time; for the Nth filler wire welding, the result of the (N-1)th welding is used as the basis for iterative calculation, and the bevel section width d after the next Nth filler wire welding is solved by iteratively solving the simultaneous equations (1), (2), and (3). N+1 Then set the swing amplitude to d. N+1 Until the filler wire welding is complete; the larger the swing amplitude, the smaller the set oscillation frequency; after each filler wire welding operation, the welding head needs to be raised by the corresponding height h. N h N The value is also obtained by iterative calculation from the simultaneous equations (1), (2), and (3); the formula for calculating the oscillation frequency is as follows: Overlap rate ;in / f, d is the swing amplitude, d is 1mm-5mm, and the overlap rate A is 50%-90%; l is the center-to-center distance, and the swing shape is circular; x is the width of the overlapping part; f is the swing frequency.

2. The laser oscillating filler wire welding method according to claim 1, characterized in that, As the wire filling process progresses, since the transverse dimension of the lower side edge of the groove cross-section increases gradually, the oscillation amplitude needs to be adjusted, and the oscillation frequency is reduced while increasing the oscillation amplitude so as to keep the energy density unchanged.

3. The laser oscillating filler wire welding method according to claim 1, characterized in that, The welding speed is 20-35 mm / s.

4. The laser oscillating filler wire welding method according to claim 1, characterized in that, The width of the bottom surface of the bevel is d1, and the bevel angle is α. In a multi-layer filler wire welding process from bottom to top, after the first layer is welded, the cross-sectional width of the bevel becomes d2, meaning the amplitude is set to d2 during the first filler wire welding. After the second layer is welded, the cross-sectional width of the bevel becomes d3, meaning the amplitude is set to d3 during the second filler wire welding, and so on. After the Nth layer is welded, the cross-sectional width of the bevel becomes d1. N+1 That is, during the Nth filler wire welding, the swing amplitude is set to d. N+1 .

5. The laser oscillating filler wire welding method according to claim 1, characterized in that, The filler wire welding process includes the following steps: a) First filler wire welding: Solve the bevel section width d2 after the first filler wire by solving equations (1), (2), and (3), and then set the swing amplitude as d2; b) Second filler wire welding: Use the result of the first welding as the basis for iterative calculation, solve the bevel section width d3 after the second filler wire by iteratively solving equations (1), (2), and (3), and then set the swing amplitude as d3; c) Third filler wire welding: Use the result of the second welding as the basis for iterative calculation, solve the bevel section width d4 after the third filler wire by iteratively solving equations (1), (2), and (3), and then set the swing amplitude as d4; d) Fourth filler wire welding: Use the result of the third welding as the basis for iterative calculation, solve the bevel section width d5 ​​after the fourth filler wire by iteratively solving equations (1), (2), and (3), and then set the swing amplitude as d5. 5。

Citation Information

Patent Citations

  • Welding path planning method and system for V-shaped groove robot

    CN110052692A

  • Groove welding method

    CN114669834A