Antiblocking agents for olefin polymerization systems, methods, and uses
By using oxygen, nitrogen, sulfur, silicon, and phosphorus compounds as anti-sticking agents in olefin polymerization reactions, the charge density and coordination space of the catalyst active sites are altered, thus solving problems such as sticking to the reactor, increasing the molecular weight of the polymer, and ensuring the smooth progress of the polymerization process.
Patent Information
- Application Number
- CN202210971764.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-12
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-08-12
AI Technical Summary
In the process of olefin polymerization, problems such as sticking to the reactor, sticking to the stirrer, and sticking to the pipe frequently occur. Existing technologies mainly solve these problems by developing new catalysts, but their universality is poor.
Oxygen-, nitrogen-, sulfur-, silicon-, and phosphorus-containing compounds are used as anti-sticking agents. These compounds are brought into contact with existing catalysts to change the charge density and coordination space of the active sites, thereby reducing the formation of low molecular weight polyolefins.
It effectively solves problems such as sticking to the reactor, improves the olefin polymerization process, increases the molecular weight of polymers, avoids adhesion to the inner wall and accessories of the reactor, and ensures smooth polymerization.
Smart Images

Figure CN117624415B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of olefin polymerization materials, specifically relating to olefin polymerization reaction systems, olefin polymerization reaction methods, and anti-sticking agents used. Background Technology
[0002] Polyolefins include polyethylene, polypropylene, polyvinyl chloride, and polystyrene. Polyethylene is the simplest general-purpose thermoplastic resin and elastomer obtained by the polymerization of ethylene monomers under the action of initiators or catalysts. Polyethylene products come in many varieties and grades to meet the needs of different fields. Polypropylene mainly consists of isotactic polypropylene (iPP) and its copolymers. The primary catalyst for synthesizing polyolefins is the highly efficient supported Ziegler-Natta catalyst, used for coordination polymerization. Another type of coordination polymerization uses metallocene catalysts, restricted geometry metallocene catalysts (CGC), and non-metallocene catalysts. In particular, metallocene catalysts, including CGC catalysts, are used to homopolymerize or copolymerize olefins such as ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, or norbornene to prepare mPE, POE, mPP, COC, EPDM, EPR, POP, PMP, OBC, etc., which have been widely used in industry worldwide and have also seen rapid development in my country's industrial sector.
[0003] However, a serious problem currently encountered in the industrial coordination polymerization of metallocene polyolefins is that during the synthesis of polyolefins using metallocene catalysts, restricted geometry metallocene catalysts (CGC), non-metallocene catalysts, and supported metallocene or non-metallocene catalysts, adhesion to the reactor, agitator, other accessories, or pipes is easily observed. This is mainly due to the production of low molecular weight polyolefins during polymerization. Polyolefins are plastics or elastomers that easily adhere to the reactor walls, agitators, or other accessories, severely affecting mass transfer, heat transfer, and flow rate, often causing product agglomeration or even charring, forcing production shutdowns.
[0004] In the current field of coordination polymerization, there are limited methods to solve the problem of polyolefin products sticking to the reactor without changing the polymerization process. Patent US20120046426 discloses that adding hydrocarbon / hydroxyl magnesium compounds during olefin polymerization can effectively reduce sticking. Patent CN105542039A discloses that a supported Ziegler-Natta catalyst can catalyze the production of polymers with good particle morphology, high bulk density, and low fine powder content, and that these polymers do not adhere to the reactor walls. Patent CN108727527A discloses a novel supported metallocene catalyst that can also produce non-stick polyolefin products.
[0005] As can be seen from the above, the main approach to solving the problem of sticking to the reactor in this field is to develop new catalysts, but the components that prevent sticking in the catalyst have not been summarized, resulting in poor universality. Summary of the Invention
[0006] The main objective of this invention is to provide an olefin polymerization reaction system, method, and anti-sticking agent. The anti-sticking agent of this invention is universal and can be used in conjunction with any catalyst in the prior art for olefin polymerization reactions to solve problems such as sticking to the reactor, stirring device, other accessories, or pipe blockage.
[0007] To achieve the above objectives, the present invention provides an anti-sticking agent for olefin polymerization reaction systems, wherein the anti-sticking agent comprises at least one selected from oxygen-containing compounds, nitrogen-containing compounds, sulfur-containing compounds, silicon-containing compounds, and phosphorus-containing compounds, wherein the general formula of the oxygen-containing compound is Formula I, the general formula of the nitrogen-containing compound is Formula II, the general formula of the sulfur-containing compound is Formula III, the general formula of the silicon-containing compound is Formula IV, and the general formula of the phosphorus-containing compound is Formula V or Formula VI.
[0008]
[0009] Among them, -R 1 -R 2 It is a hydrocarbon group with a total carbon number between 8 and 60;
[0010] -R 3 -R 4 -R 5 It is a -H or hydrocarbon group, with a total carbon number between 8 and 60;
[0011] -R 6 -R 7 It is a -H or hydrocarbon group, with a total carbon number between 8 and 60;
[0012] -R 8 -R 9 -R 10 -R 11 It is a hydrocarbon group or hydrocarbon oxygen group, with a total carbon number between 8 and 60;
[0013] -R 12 -R 13 -R 14 It is -H, hydrocarbon group or hydrocarbon oxygen group, and the total number of carbons is between 8 and 60.
[0014] The anti-sticking agent for olefin polymerization reaction systems described in this invention, wherein R 1 and -R 2 The total carbon number is between 8 and 30, -R 3 -R 4 -R 5The total carbon number is between 8 and 30, -R 6 -R 7 The total carbon number is between 8 and 30, -R 8 -R 9 -R 10 -R 11 The total carbon number is between 8 and 30, -R 12 -R 13 -R 14 The total carbon number is between 8 and 30.
[0015] The anti-sticking agent for olefin polymerization reaction systems according to the present invention comprises, wherein the oxygen-containing compound is selected from at least one of dibutyl ether, dipentyl ether, dihexyl ether, diheptyl ether, and diphenyl ether; and the silicon-containing compound is selected from methyldimethoxycyclohexylsilane, methyldimethoxycyclopentylsilane, trimethoxycyclohexylsilane, trimethoxycyclopentoxysilane, trimethoxycyclohexylsilane, ethyldimethoxycyclohexylsilane, methyldiethoxycyclohexylsilane, methyldiethoxycyclopentylsilane, methyldiethoxycyclohexylsilane, methyldiethoxycyclohexylsilane, methyldimethoxycyclopentoxysilane, dimethylethoxycyclohexylsilane, dimethylmethoxycyclohexylsilane, dimethylmethoxycyclopentylsilane, dimethylethoxycyclohexylsilane, dimethylethoxycyclopentoxysilane, dimethylethoxycyclopentoxysilane, cyclohexylmethyldimethoxysilane. At least one of dicyclopentyldimethoxysilane; the phosphorus-containing compound is selected from at least one of tributyl phosphate, tricyclopentyl phosphate, dibutyl phosphite, 2-ethylhexyl phosphate, tributylphosphine, tricyclohexylphosphine, tri-n-butylphosphine, and trihexylphosphine oxide; the sulfur-containing compound is selected from at least one of dipentyl disulfide, 1,9-nonanedithiol, n-dodecylthiol, bis(16-hydroxyhexadecyl)disulfide, and dicyclohexyl disulfide; the nitrogen-containing compound is selected from at least one of tripentylamine, dihexylamine, dicyclohexylamine, spermine, spermidine, decanediamine, 3-propylpiperidine, 4-piperidinylpiperidine, (1-cyclopropylpyrrolidine-3-yl)methylamine, N,N,N′,N′-tetramethyl-1,6-hexanediamine, N-propylcyclohexylamine, and N,N-dimethylcyclohexylamine.
[0016] To achieve the above objectives, the present invention also provides an olefin polymerization reaction system in which the above-mentioned anti-sticking agent is added.
[0017] To achieve the above objectives, the present invention further provides an olefin polymerization method, wherein the olefin polymerization method uses olefins as raw materials and carries out the polymerization reaction under the action of a catalyst and the aforementioned anti-sticking agent.
[0018] In the olefin polymerization method of the present invention, the anti-sticking agent is added during the preparation or formulation of the catalyst, or the anti-sticking agent and the catalyst are added during the olefin prepolymerization process.
[0019] The olefin polymerization method of the present invention includes a catalyst that is a metallocene catalyst, a restricted geometry metallocene catalyst, a non-metallocene catalyst, a supported metallocene catalyst, a supported restricted geometry metallocene catalyst, or a supported non-metallocene catalyst.
[0020] The olefin polymerization method of the present invention includes a solution polymerization reaction, a gas-phase polymerization reaction, a liquid-phase bulk polymerization reaction, a slurry polymerization reaction, a loop polymerization reaction, or a combination polymerization reaction.
[0021] The olefin polymerization method of the present invention includes the following steps:
[0022] Step 1: Ensure the catalyst and the anti-sticking agent are in full contact;
[0023] Step 2: Mix the co-catalyst with the mixture obtained in Step 1;
[0024] Step 3: Under the action of the mixture obtained in step 2, the olefin undergoes a polymerization reaction.
[0025] The olefin polymerization method of the present invention, wherein the catalyst is a transition metal, the molar ratio of the catalyst to the anti-sticking agent is 1:0.01-2, and the molar ratio of the catalyst to the co-catalyst is 1:10-1000; the co-catalyst is selected from at least one of trimethylaluminum, triethylaluminum, tripropylaluminum, triisobutylaluminum, tri-n-hexylaluminum, tri-tert-butylaluminum, trioctylaluminum, diethylaluminum chloride, diethylaluminum chloride, sesquiethylaluminum chloride, methoxyaluminum, and modified methoxyaluminum.
[0026] The olefin polymerization method of the present invention includes ethylene polymerization, propylene polymerization, copolymerization of ethylene with other organic compounds containing carbon-carbon double bonds, and copolymerization of propylene with other organic compounds containing carbon-carbon double bonds, wherein the other organic compounds containing carbon-carbon double bonds are selected from C2-C4. 30 α-olefins, C6-C 30 dienes, C3-C 100 Oxygen-containing organic compounds containing carbon-carbon double bonds, wherein the C2-C 30 The α-olefin is selected from ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, dicyclopentadiene, norbornene, or mixtures thereof, wherein the C3-C 100 The oxygen-containing organic compounds containing carbon-carbon double bonds are preferably 7-octen-1-ol, 9-decen-1-ol or mixtures thereof.
[0027] The olefin polymerization method of the present invention includes a polymerization reaction temperature of 20-200℃, a time of 5-300 min, and a gas pressure of 0.05-40 MPa.
[0028] The beneficial effects of this invention are:
[0029] The heteroatoms (oxygen, nitrogen, sulfur, silicon, phosphorus) of the anti-sticking agent of this invention can contact the active sites of the catalyst used for olefin polymerization. Due to the high electronegativity of the heteroatoms, the charge density distribution of the central transition metal atom at the active site of the catalyst is changed, thus altering the electronic effect of the active site. Furthermore, because the heteroatoms of the anti-sticking agent contact the active site of the catalyst, the distance between the anti-sticking agent molecules and the active site is very close. The anti-sticking agent molecules change the coordination space of the active site, that is, they change the coordination environment of the olefin. This reduces the content of low molecular weight polyolefins obtained from olefin polymerization, thereby obtaining higher molecular weight polyolefins. The polyolefin product does not stick in the polymerization reactor, improving problems such as sticking to the reactor, agitator, other accessories, or pipe blockage during the olefin polymerization process. Attached Figure Description
[0030] Figure 1 The sticking situation of the reactor when the anti-sticking agent of the present invention is added to the olefin polymerization system.
[0031] Figure 2 This refers to the sticking situation in the olefin polymerization system when the anti-sticking agent of this invention was not added. Detailed Implementation
[0032] The technical solution of the present invention will be described in detail below. The following embodiments are implemented under the premise of the technical solution of the present invention and a detailed implementation process is given. However, the protection scope of the present invention is not limited to the following embodiments. Structures or experimental methods that do not specify specific conditions in the following embodiments are generally performed under conventional conditions.
[0033] This invention provides an anti-sticking agent for olefin polymerization reaction systems. The anti-sticking agent comprises at least one selected from oxygen-containing compounds, nitrogen-containing compounds, sulfur-containing compounds, silicon-containing compounds, and phosphorus-containing compounds. The oxygen-containing compound has the general formula I, the nitrogen-containing compound has the general formula II, the sulfur-containing compound has the general formula III, the silicon-containing compound has the general formula IV, and the phosphorus-containing compound has the general formula V or VI.
[0034]
[0035] Among them, -R 1 -R 2 It is a hydrocarbon group with a total carbon number between 8 and 60;
[0036] -R 3 -R4 -R 5 It is a -H or hydrocarbon group, with a total carbon number between 8 and 60;
[0037] -R 6 -R 7 It is a -H or hydrocarbon group, with a total carbon number between 8 and 60;
[0038] -R 8 -R 9 -R 10 -R 11 It is a hydrocarbon group or hydrocarbon oxygen group, with a total carbon number between 8 and 60;
[0039] -R 12 -R 13 -R 14 It is -H, hydrocarbon group or hydrocarbon oxygen group, and the total number of carbons is between 8 and 60.
[0040] The heteroatoms (oxygen, nitrogen, sulfur, silicon, and phosphorus) of the anti-sticking agent of this invention can contact the active sites of catalysts used in olefin polymerization in the prior art. Due to the high electronegativity of the heteroatoms, the charge density distribution of the central transition metal atom at the catalyst active site is altered, thus changing the electronic effect of the catalyst active site. Furthermore, because the heteroatoms of the anti-sticking agent contact the catalyst active site, the distance between the anti-sticking agent molecules and the catalyst active site is very close, altering the coordination space of the catalyst active site. Therefore, the anti-sticking agent of this invention can change the coordination environment of olefins, resulting in a reduction in the content of low molecular weight polyolefins obtained from olefin polymerization. More importantly, it improves problems such as sticking to the reactor, agitator, other accessories, or pipes during the olefin polymerization process.
[0041] In one embodiment, in the anti-adhesion agent of the present invention, R 1 and -R 2 The total carbon number is between 8 and 30, more preferably between 8 and 20, -R 3 -R 4 -R 5 The total carbon number is between 8 and 30, more preferably between 8 and 20, -R 6 -R 7 The total carbon number is between 8 and 30, more preferably between 8 and 20, -R 8 -R 9 -R 10 -R 11 The total carbon number is between 8 and 30, more preferably between 8 and 20, -R 12 -R 13 -R 14 The total carbon number is between 8 and 30, more preferably between 8 and 20.
[0042] Among them, oxygen-containing compounds are, for example, ethers or oxo compounds; sulfur-containing compounds are, for example, thioethers, thiols, or thio compounds; nitrogen-containing compounds are, for example, amine compounds; silicon-containing compounds are, for example, silane compounds; and phosphorus-containing compounds are, for example, phosphine, phosphine oxide, or (phosphite) esters.
[0043] In another embodiment, the oxygen-containing compound of the present invention is selected from at least one of dibutyl ether, dipentyl ether, dihexyl ether, diheptyl ether, and diphenyl ether; the silicon-containing compound is selected from methyldimethoxycyclohexylsilane, methyldimethoxycyclopentylsilane, trimethoxycyclohexylsilane, trimethoxycyclopentoxysilane, trimethoxycyclohexylsilane, ethyldimethoxycyclohexylsilane, methyldiethoxycyclohexylsilane, methyldiethoxycyclopentylsilane, methyldiethoxycyclohexylsilane, methyldiethoxycyclohexylsilane, methyldimethoxycyclopentoxysilane, dimethylethoxycyclohexylsilane, dimethylmethoxycyclohexylsilane, dimethylmethoxycyclopentylsilane, dimethylethoxycyclohexylsilane, dimethylethoxycyclopentoxysilane, dimethylethoxycyclopentoxysilane, cyclohexylmethyldimethoxysilane, dicyclopentyl ... The compound is selected from at least one of the following: silanes; the phosphorus-containing compound is selected from at least one of the following: tributyl phosphate, tricyclopentyl phosphate, dibutyl phosphite, 2-ethylhexyl phosphate, tributylphosphine, tricyclohexylphosphine, tri-n-butylphosphine, and trihexylphosphine oxide; the sulfur-containing compound is selected from at least one of the following: dipentyl disulfide, 1,9-nonanedithiol, n-dodecyl mercaptan, bis(16-hydroxyhexadecyl) disulfide, and dicyclohexyl disulfide; the nitrogen-containing compound is selected from at least one of the following: tripentylamine, dihexylamine, dicyclohexylamine, spermine, spermidine, decanediamine, 3-propylpiperidine, 4-piperidinylpiperidine, (1-cyclopropylpyrrolidine-3-yl)methylamine, N,N,N′,N′-tetramethyl-1,6-hexanediamine, N-propylcyclohexylamine, and N,N-dimethylcyclohexylamine.
[0044] Adding the anti-sticking agent described above to the olefin polymerization reaction system allows the anti-sticking agent to come into contact with the catalyst used for olefin polymerization. This can change the electronic effect and coordination space of the catalyst's active sites, thereby reducing the content of low molecular weight polyolefins obtained from olefin polymerization and improving problems such as sticking to the reactor in the polymerization system.
[0045] In one embodiment, the anti-sticking agent of the present invention is added during the preparation or formulation of the catalyst used for olefin polymerization; that is, the anti-sticking agent is added during the preparation or formulation of the catalyst for olefin polymerization to bring the anti-sticking agent into contact with the catalyst. In another embodiment, the anti-sticking agent and the catalyst of the present invention are added during the olefin prepolymerization process; that is, the anti-sticking agent and the catalyst of the present invention are added simultaneously or sequentially during the olefin prepolymerization process to bring the anti-sticking agent into contact with the catalyst. In yet another embodiment, the anti-sticking agent and the catalyst of the present invention may also be mixed first and then added to the olefin polymerization system.
[0046] In one embodiment, the olefin polymerization method of the present invention includes the following steps:
[0047] Step 1: Ensure the catalyst and anti-sticking agent are in full contact;
[0048] Step 2: Mix the co-catalyst with the mixture obtained in Step 1;
[0049] Step 3: Under the action of the mixture obtained in step 2, the olefin undergoes a polymerization reaction.
[0050] This invention does not impose any particular limitation on the catalyst, as long as it can be used for olefin polymerization. Examples include metallocene catalysts, confined geometry metallocene catalysts (CGC), non-metallocene catalysts, supported metallocene catalysts, supported confined geometry metallocene catalysts (CGC), or supported non-metallocene catalysts. The anti-sticking agent described in this invention, during contact with the catalyst, alters the electronic effects and coordination space of the active sites in the catalyst, thereby reducing the content of low molecular weight polyolefins obtained from olefin polymerization.
[0051] In one embodiment, the catalyst of the present invention is based on a transition metal, and the molar ratio of the catalyst to the anti-sticking agent is 1:0.01-2. The contact temperature between the catalyst and the anti-sticking agent is -20 to 60°C, and stirring is performed during the contact process for 0.1 to 20 hours.
[0052] Then, the co-catalyst is mixed with the mixture obtained in step 1 to catalyze the polymerization reaction of olefins.
[0053] This invention does not specifically limit the type of polymerization reaction, such as solution polymerization, gas-phase polymerization, liquid-phase bulk polymerization, slurry polymerization, loop polymerization, or combined polymerization. Furthermore, this invention does not specifically limit the olefins, and can include ethylene polymerization, propylene polymerization, copolymerization of ethylene with other organic compounds containing carbon-carbon double bonds, copolymerization of propylene with other organic compounds containing carbon-carbon double bonds, thereby synthesizing polyolefin materials, flame-retardant polyolefin materials, and functionalized polyolefin materials. The other organic compounds containing carbon-carbon double bonds are selected from C2-C... 30 α-olefins, C6-C 30 dienes, C3-C 100 Oxygen-containing organic compounds containing carbon-carbon double bonds; wherein the C2-C 30 The olefin is preferably selected from ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, dicyclopentadiene, norbornene, or mixtures thereof; C3-C 100 The oxygen-containing organic compounds containing carbon-carbon double bonds are preferably 7-octen-1-ol, 9-decen-1-ol, or mixtures thereof.
[0054] In one embodiment, the polymerization reaction temperature is 20-200℃, the reaction time is 5-300 min, and the gas pressure is 0.05-40 MPa to obtain the product; wherein the obtained product is a high-end polyolefin material, which may be mPE, POE, mPP, COC, COP, EPDM, EPR, POP, PMP, OBC, etc.
[0055] In one specific embodiment, the olefin polymerization reaction method of the present invention includes the following steps:
[0056] (1) In a preparation tank for a supported catalyst, a preparation tank for a homogeneous catalyst, a preparation tank for a supported catalyst, or an olefin prepolymerization tank, an organic solvent is added, followed by the catalyst and an anti-sticking agent. The mixture is stirred at -20 to 60°C for 0.1 to 20 hours to ensure sufficient contact between the active sites of the catalyst and the anti-sticking agent molecules. The catalyst can be a metallocene catalyst, a restricted geometry metallocene catalyst (CGC), a non-metallocene catalyst, a supported metallocene catalyst, a supported restricted geometry metallocene catalyst (CGC), or a supported non-metallocene catalyst. The anti-sticking agent can be any of the above-mentioned anti-sticking agents. The organic solvent is selected from C5-C64. 50 saturated hydrocarbons, C5-C 50 Alicyclic hydrocarbons, C6-C 50 Aromatic hydrocarbons or C3-C 50 The solvent is a saturated heterocyclic hydrocarbon or paraffin oil or a mixture thereof, preferably toluene, xylene, diphenyl ether, biphenyl, hexane, heptane, octane, decane, cyclohexane, petroleum ether, paraffin oil, white oil, dodecane, tetradecane or hexadecane, or a mixture thereof; the molar ratio of the transition metal to the anti-sticking agent in the catalyst is 1:0.01-2.
[0057] (2) At -20-60℃, add a co-catalyst to the mixture obtained in step (1), wherein the molar ratio of transition metal to co-catalyst in the catalyst is 1:10-1000, and stir for 10-600 min; wherein the co-catalyst is alkyl aluminum, alkoxy aluminum or a mixture thereof; further, the co-catalyst is selected from trimethyl aluminum, triethyl aluminum, tripropyl aluminum, triisobutyl aluminum, tri-n-hexyl aluminum, tri-tert-butyl aluminum, trioctyl aluminum, diethylaluminum chloride, diethylaluminum chloride, sesquiethylaluminum chloride, MAO or modified MAO, etc., and can be used alone or in combination.
[0058] (3) Add the catalyst prepared in step (2) to the polymerization reactor, add an organic solvent, and use the catalyst to catalyze the polymerization of ethylene, the polymerization of propylene, the copolymerization of ethylene with other organic compounds containing carbon-carbon double bonds, and the copolymerization of propylene with other organic compounds containing carbon-carbon double bonds to synthesize polyolefin materials, flame-retardant polyolefin materials, and functionalized polyolefin materials, wherein the other organic compounds containing carbon-carbon double bonds are selected from C2-C4. 30α-olefins, C6-C 30 dienes, C3-C 100 Oxygen-containing organic compounds containing carbon-carbon double bonds; wherein the C2-C 30 The olefin is preferably selected from ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, dicyclopentadiene, norbornene, or mixtures thereof; C3-C 100 The preferred oxygen-containing organic compounds with carbon-carbon double bonds are 7-octen-1-ol, 9-decen-1-ol, or mixtures thereof; the polymerization temperature is maintained at 20-200℃, the reaction time is 5-300 min, and the gas pressure is 0.05-40 MPa to obtain the product; the polymerization process used is solution polymerization, gas-phase polymerization, liquid-phase bulk polymerization, slurry polymerization, loop polymerization, or combined polymerization; the resulting product is a high-end polyolefin material, such as mPE, POE, mPP, COC, COP, EPDM, EPR, POP, PMP, OBC, etc.
[0059] When performing olefin polymerization, the organic solvent used is selected from C5-C4. 50 saturated hydrocarbons, C5-C 50 Alicyclic hydrocarbons, C6-C 50 Aromatic hydrocarbons or C3-C 50 The solvent is a saturated heterocyclic hydrocarbon or paraffin oil or a mixture thereof, preferably toluene, xylene, diphenyl ether, biphenyl, hexane, heptane, octane, decane, cyclohexane, petroleum ether, paraffin oil, white oil, dodecane, tetradecane or hexadecane, or a mixture thereof.
[0060] Therefore, this invention relates to the homopolymerization or copolymerization of ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, or norbornene using metallocene catalysts, restricted geometry metallocene catalysts (CGC), non-metallocene catalysts, supported metallocene catalysts, or supported non-metallocene catalysts to prepare mPE, POE, mPP, COC, COP, EPDM, EPR, POP, PMP, OBC, etc. Anti-sticking agents, such as oxygen-containing compounds, nitrogen-containing compounds, sulfur-containing compounds, silicon-containing compounds, and phosphorus-containing compounds, are added during catalyst preparation or olefin prepolymerization. This prevents the reaction system from sticking to the reactor, stirrer, other accessories, and pipes. Furthermore, the olefin polymerization method using anti-sticking agents of this invention is simple, low-cost, requires minimal equipment, consumes little energy, and causes minimal environmental pollution.
[0061] The technical solution of the present invention will be further described in detail below through specific embodiments. Wherein, the content in parentheses, such as "0.1wt% hexane solution," means that the solute is added in the form of a hexane solution containing a solute concentration of 0.1wt%. Furthermore, the anti-sticking agent of the present invention is generally a commercially available product; for the synthesis of some alkoxysilane compounds, please refer to patent CN106317268A.
[0062] Example 1
[0063] (1) Dry the catalyst preparation vessel and purge it with nitrogen. At -20°C, add 20 mL of n-hexane, 30 mg of dimethylcyclopentadiene titanium trichloride, and 0.12 mL of dimethylmethoxycyclohexylsilane (0.1 wt% hexane solution) as an anti-sticking agent. Stir for 6 minutes, add 6 mL of MAO (10 wt% toluene solution), and stir for 600 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 2 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 20°C. Purge with 0.1 L of hydrogen and ethylene until the pressure is 0.05 MPa. Stir and react for 30 minutes. Collect 11 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 33 × 10⁻⁶. 4 g / mol.
[0064] Example 2
[0065] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 10 mL of n-hexane, 20 mg of dimethylsilyldiindene titanium dichloride, and 0.8 mL of methyldiethoxycyclohexyloxysilane (1 wt% hexane solution) as an anti-sticking agent to the catalyst preparation vessel at 30°C. Stir for 30 minutes. Add 5 mL of MAO (10 wt% toluene solution) and stir for 30 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 3 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 25°C. Add 0.2 L of propylene and ethylene to a pressure of 0.9 MPa. Stir and heat to 55°C for 30 minutes. Collect 122 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 52 × 10⁻⁶. 4 g / mol.
[0066] Example 3
[0067] (1) Dry the catalyst preparation tank and purge it with nitrogen. Add 30 mL of n-hexane, 30 mg of dimethylsilylaniline cyclopentadiene titanium dichloride, and 2.4 mL of methyldimethoxycyclohexylsilane (1 wt% toluene solution) as an anti-sticking agent to the catalyst preparation tank at 60°C. Stir for 40 minutes. Add 40 mL of MAO (10 wt% toluene solution) and stir for 300 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 2 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 60°C. Add 0.1 L of propylene, 30 mL of 1-octene, and ethylene to a pressure of 8 MPa. Stir and heat to 160°C for 5 minutes. Collect 26 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 12 × 10⁻⁶. 4 g / mol.
[0068] Example 4
[0069] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 30 mL of n-hexane, 30 mg of dimethylsilyl-2,6-difluoroaniline-cyclopentadiene titanium dichloride, and 0.2 mL of dipentyl ether (1 wt% heptane solution) to the catalyst preparation vessel at 30 °C. Stir for 60 minutes. Add 8 mL of MAO (10% toluene solution) and stir for 60 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 2 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 30 °C. Add 30 mL of 1-octene and ethylene to a pressure of 1.5 MPa. Stir and heat to 145 °C for 20 minutes. Collect 55 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 115 × 10⁻⁶. 4 g / mol.
[0070] Example 5
[0071] (1) Dry the catalyst preparation tank and purge it with nitrogen. Add 20 mL of n-hexane to the catalyst preparation tank at 40°C, add 30 mg of silica-supported dimethylsilylaniline cyclopentadiene titanium dichloride (titanium content 1.5 wt%), add 1.2 mL of trimethoxycyclohexyloxysilane (1 wt% hexane solution) as an anti-sticking agent, and stir for 300 minutes; add 0.3 mL of triethylaluminum (1.5 M hexane solution), and stir for 300 minutes; (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 5 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 40°C, add 10 mL of 1-butene, add ethylene to the pressure of 25 MPa, stir, heat to 200°C and react for 90 minutes, collect 131 g of the polymerization product, with a weight average molecular weight of 52 × 10⁻⁶. 4 g / mol, non-stick reactor.
[0072] Example 6
[0073] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane, 15 mg of α-diimide nickel dibromide, and 0.15 mL of cyclohexylmethyldimethoxysilane (1 wt% hexane solution) to the catalyst preparation vessel at -20℃ and stir for 30 minutes. Add 7 mL of MAO (10% toluene solution) and stir for 30 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 3 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 30℃. Add 10 mL of styrene and ethylene to a pressure of 0.8 MPa, stir, and heat to 50℃ for 30 minutes. Collect 35 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 46 × 10⁻⁶. 4 g / mol.
[0074] Example 7
[0075] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane, 15 mg of α-diimide nickel dibromide, and 0.25 mL of tricyclopentyl phosphate (1 wt% hexane solution) as an anti-sticking agent to the catalyst preparation vessel at 30°C. Stir for 30 minutes. Add 15 mL of MAO (10% toluene solution) and stir for 30 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 3 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 30°C. Add 10 mL of propylene and ethylene to a pressure of 0.8 MPa. Stir and heat to 50°C for 30 minutes. Collect 46 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 49 × 10⁻⁶. 4 g / mol.
[0076] Example 8
[0077] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane, 15 mg of α-diimide nickel dibromide, and 1.3 mL of tripentylamine (1 wt% hexane solution) to the catalyst preparation vessel at 10 °C. Stir for 20 hours. Add 15 mL of MAO (10% toluene solution) and stir for 600 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 3 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 30 °C. Add 10 mL of propylene and ethylene until the pressure is 0.05 MPa. Stir and maintain the reaction at 10 °C for 300 minutes. Collect 52 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 44 × 10⁻⁶. 4 g / mol.
[0078] Example 9
[0079] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane, 15 mg of α-diimide nickel dibromide, and 0.1 mL of dipentyl disulfide (1 wt% hexane solution) to the catalyst preparation vessel at 30°C and stir for 30 minutes. Add 15 mL of MAO (10% toluene solution) and stir for 30 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 3 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 30°C. Add 10 mL of propylene and ethylene to a pressure of 0.8 MPa, stir, and heat to 50°C for 30 minutes. Collect 41 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 43 × 10⁻⁶. 4 g / mol.
[0080] Example 10
[0081] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane, 15 mg of FI titanium catalyst, and 0.1 mL of anti-sticking agent ethyl dimethoxycyclohexylsilane (1 wt% hexane solution) to the catalyst preparation vessel at 60°C and stir for 30 minutes. Add 15 mL of MAO (10% toluene solution) and stir for 30 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 3 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 30°C. Add 10 mL of propylene and ethylene to a pressure of 0.8 MPa, stir, and heat to 80°C for 30 minutes. Collect 57 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 45 × 10⁻⁶. 4 g / mol.
[0082] Example 11
[0083] (1) Dry the catalyst preparation tank and purge it with nitrogen. Add 20 mL of n-hexane, 15 mg of FI titanium catalyst, and 2 mL of anti-sticking agent ethyl dimethoxycyclohexylsilane (1 wt% hexane solution) to the catalyst preparation tank at 60°C and stir for 10 hours. Add 15 mL of MAO (10% toluene solution) and stir for 300 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 3 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 60°C. Add 10 mL of propylene and ethylene to a pressure of 40 MPa, stir, and heat to 140°C for 15 minutes. Collect 94 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 37 × 10⁻⁶. 4 g / mol.
[0084] Example 12
[0085] (1) Dry the catalyst preparation tank and purge it with nitrogen. Add 20 mL of n-hexane, 15 mg of FI titanium catalyst, and 0.5 mL of anti-sticking agent ethyl dimethoxycyclohexylsilane (1 wt% hexane solution) to the catalyst preparation tank at 60°C and stir for 20 hours. Add 7.5 mL of MAO (10% toluene solution) and stir for 600 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 3 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 60°C. Add 10 mL of propylene and ethylene to a pressure of 20 MPa, stir, and heat to 200°C for 5 minutes. Collect 64 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 31 × 10⁻⁶. 4 g / mol.
[0086] Example 13
[0087] (1) Dry the catalyst preparation tank and purge it with nitrogen. Add 20 mL of n-hexane to the catalyst preparation tank at 30°C, add 30 mg of silica-supported α-diimide titanium dichloride (titanium content 1.1 wt%), add 0.1 mL of anti-sticking agent trimethoxycyclohexyloxysilane (1 wt% hexane solution), and stir for 30 minutes; add 5.5 mL of MAO (10% toluene solution), and stir for 30 minutes; (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 5 mL of the catalyst prepared in step (1) and add it to the 2-liter stainless steel autoclave at 30°C, add 10 mL of 1-butene, add ethylene to the pressure of 0.8 MPa, stir, heat to 65°C and react for 90 minutes, collect 37 g of polymerization product with a weight average molecular weight of 51 × 10⁻⁶. 4 g / mol, non-stick reactor.
[0088] Example 14
[0089] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane, 20 mg of aniline diphenylphosphine dichloride titanium catalyst, and 1 mL of dicyclopentyl dimethoxysilane (1 wt% hexane solution) as an anti-sticking agent to the catalyst preparation vessel at 30°C. Stir for 30 minutes. Then add 15 mL of MAO (10% toluene solution) and stir for 30 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, add all the catalyst prepared in step (1) to the 2-liter stainless steel autoclave at 30°C. Add 5 mL of 9-decen-1-ol, heat to 50°C, and add ethylene to a pressure of 0.8 MPa. Stir for 30 minutes and collect 15 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 50 × 10⁻⁶. 4 g / mol.
[0090] Example 15
[0091] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane, 20 mg of 2,4,6-trimethylaniline diphenylphosphine titanium dichloride catalyst, and 0.1 mL of dicyclopentyldimethoxysilane (0.1 wt% hexane solution) as an anti-sticking agent to the catalyst preparation vessel at 30°C. Stir for 20 hours. Add 15 mL of MAO (10% toluene solution) and stir for 100 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, add all the catalyst prepared in step (1) to the 2-liter stainless steel autoclave at 30°C. Add 5 mL of 9-decen-1-ol, cool to 0°C, and add ethylene to a pressure of 0.05 MPa. Stir for 30 minutes and collect 5 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 52 × 10⁻⁶. 4 g / mol.
[0092] Example 16
[0093] (1) Dry the catalyst preparation vessel and purge it with nitrogen. At 30°C, add 20 mL of n-hexane, 20 mg of 2,6-difluoroaniline-dicyclohexylphosphine titanium dichloride catalyst, 15 mL of MAO (10% toluene solution), and 1 mL of dicyclopentyldimethoxysilane (1 wt% hexane solution) as an anti-sticking agent. Stir for 30 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, add all the catalyst prepared in step (1) to the 2-liter stainless steel autoclave at 30°C. Add 5 mL of 9-decen-1-ol, heat to 40°C, and add ethylene to a pressure of 0.8 MPa. Stir for 30 minutes and collect 15 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 45 × 10⁻⁶. 4 g / mol.
[0094] Example 17
[0095] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane, 20 mg of 2,4,6-trifluoroaniline dicyclohexylphosphine titanium dichloride catalyst, and 30 mL of MAO (10% toluene solution) to the catalyst preparation vessel at 30°C. Stir for 10 minutes, then add 0.1 mL of dicyclopentyldimethoxysilane (1 wt% hexane solution) as an anti-sticking agent and stir for 20 hours. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, add all the catalyst prepared in step (1) to the 2-liter stainless steel autoclave at 30°C. Add 5 mL of 9-decen-1-ol, heat to 70°C, and add ethylene to a pressure of 0.3 MPa. Stir for 5 minutes and collect 8 g of the polymerization product. The product does not stick to the autoclave and has a weight-average molecular weight of 43 × 10⁻⁶. 4 g / mol.
[0096] Example 18
[0097] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane, 20 mg of 2,6-difluoroaniline dicyclohexylphosphine titanium dichloride catalyst, and 5 mL of MAO (10% toluene solution) to the catalyst preparation vessel at 30°C. Stir for 600 minutes, then add 0.5 mL of dicyclopentyldimethoxysilane (1 wt% hexane solution) as an anti-sticking agent and stir for 10 hours. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, add all the catalyst prepared in step (1) to the 2-liter stainless steel autoclave at 30°C, add 5 mL of 9-decen-1-ol, cool to -20°C, add ethylene to a pressure of 12 MPa, stir for 300 minutes, collect 38 g of the polymerization product, which does not stick to the autoclave, and has a weight-average molecular weight of 83 × 10⁻⁶. 4 g / mol.
[0098] Comparative Example 1
[0099] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane and 15 mg of FI titanium catalyst to the catalyst preparation vessel at 30 °C and stir for 30 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 3 mL of the prepared catalyst and add it to the 2-liter stainless steel autoclave at 30 °C. Add 15 mL of MAO (10% toluene solution), 10 mL of propylene, and ethylene until the pressure reaches 0.8 MPa. Stir and heat to 50 °C for 30 minutes. Collect 5 g of the polymerization product. The product sticks to the vessel and has a weight-average molecular weight of 7.5 × 10⁻⁶. 4 g / mol.
[0100] Comparative Example 2
[0101] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane and 15 mg of α-diimide nickel dibromide to the catalyst preparation vessel at 30 °C and stir for 30 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 3 mL of the prepared catalyst and add it to the 2-liter stainless steel autoclave at 30 °C. Add 15 mL of MAO (10% toluene solution), add 10 mL of propylene, and add ethylene until the pressure is 0.8 MPa. Stir and heat to 50 °C to react for 30 minutes. Collect 4 g of the polymerization product. The product sticks to the vessel and has a weight-average molecular weight of 6.5 × 10⁻⁶. 4 g / mol.
[0102] Comparative Example 3
[0103] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 30 mL of n-hexane and 30 mg of dimethylsilyl-2,6-difluoroaniline-cyclopentadiene titanium dichloride to the catalyst preparation vessel at 30 °C and stir for 60 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 2 mL of the prepared catalyst and add it to the 2-liter stainless steel autoclave at 30 °C. Add 8 mL of MAO (10% toluene solution), charge 30 mL of 1-octene, and charge ethylene to a pressure of 0.8 MPa. Stir and heat to 55 °C for 20 minutes. Collect 2 g of the polymerization product. The product sticks to the vessel and has a weight-average molecular weight of 55 × 10⁻⁶. 4 g / mol.
[0104] Comparative Example 4
[0105] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane and 30 mg of dimethylcyclopentadiene titanium trichloride to the catalyst preparation vessel at 20°C and stir for 20 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 2 mL of the prepared catalyst and add it to the 2-liter stainless steel autoclave at 20°C. Add 6 mL of MAO (10% toluene solution), purge with 0.1 L of hydrogen, and purge with ethylene until the pressure is 0.7 MPa. Stir and heat to 55°C for 1 hour. Collect 2 g of the polymerization product. The product sticks to the vessel and has a weight-average molecular weight of 3.5 × 10⁻⁶. 4 g / mol.
[0106] Comparative Example 5
[0107] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 30 mL of n-hexane and 30 mg of dimethylsilylaniline cyclopentadiene titanium dichloride to the catalyst preparation vessel at 30 °C and stir for 40 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, measure 2 mL of the prepared catalyst and add it to the 2-liter stainless steel autoclave at 30 °C. Add 8 mL of MAO (10% toluene solution), 0.1 L of propylene, 30 mL of 1-octene, 0.7 mL of the anti-sticking agent methyldimethoxycyclohexylsilane, and ethylene to a pressure of 0.8 MPa. Stir and heat to 65 °C for 30 minutes. Collect 4.5 g of the polymerization product. The product sticks to the autoclave and has a weight-average molecular weight of 25 × 10⁻⁶. 4 g / mol.
[0108] Comparative Example 6
[0109] (1) Dry the catalyst preparation vessel and purge it with nitrogen. Add 20 mL of n-hexane, 20 mg of 2,6-difluoroaniline dicyclohexylphosphine titanium dichloride catalyst, and 15 mL of MAO (10% toluene solution) to the catalyst preparation vessel at 30°C and stir for 30 minutes. (2) After fully purging the 2-liter stainless steel autoclave with nitrogen, add all the prepared catalyst to the 2-liter stainless steel autoclave at 30°C, add 5 mL of 9-decen-1-ol, heat to 40°C, add ethylene to the pressure of 0.8 MPa, stir for 30 minutes, collect 12 g of the polymerization product, which sticks to the vessel, with a weight-average molecular weight of 15 × 10⁻⁶. 4 g / mol.
[0110] As can be seen from the above embodiments and comparative examples, adding the anti-sticking agent of the present invention can improve the situation of polymer sticking during polymerization. In the present invention, "sticking" refers to the polymer adhering to the equipment in the form of filaments or powder clumps. Generally, when polymerizing in smaller equipment, sticking can be directly observed and judged during or after the reaction; when polymerizing in larger equipment, sticking can be indirectly judged by parameters such as power equipment load, or it can be directly observed and judged after polymerization.
[0111] Of course, the present invention may have other various embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications according to the present invention, but these corresponding changes and modifications should all fall within the protection scope of the claims of the present invention.
Claims
1. An anti-sticking agent for olefin polymerization reaction systems, characterized in that, The anti-sticking agent includes at least one of a nitrogen-containing compound, a sulfur-containing compound, and a phosphorus-containing compound. The nitrogen-containing compound has the general formula of Formula II, the phosphorus-containing compound has the general formula of Formula V or Formula VI, and the sulfur-containing compound is selected from at least one of dipentyl disulfide, 1,9-nonanedithiol, bis(16-hydroxyhexadecyl) disulfide, and dicyclohexyl disulfide. 、 、 Formula II, Formula V, Formula VI in, -R 3 -R 4 -R 5 It is a -H or hydrocarbon group, with a total carbon number between 8 and 60; -R 12 -R 13 -R 14 It is -H, hydrocarbon group or hydrocarbon oxygen group, and the total number of carbons is between 8 and 60.
2. The anti-sticking agent for olefin polymerization reaction systems according to claim 1, characterized in that, -R 3 -R 4 -R 5 The total carbon number is between 8 and 30, -R 12 -R 13 -R 14 The total carbon number is between 8 and 30.
3. The anti-sticking agent for olefin polymerization reaction systems according to claim 2, characterized in that, The phosphorus-containing compound is selected from at least one of tributyl phosphate, tricyclopentyl phosphate, dibutyl phosphite, 2-ethylhexyl phosphate, tributylphosphine, tricyclohexylphosphine, tri-n-butylphosphine, and trihexylphosphine oxide; the nitrogen-containing compound is selected from at least one of tripentylamine, dihexylamine, dicyclohexylamine, spermine, spermidine, decanediamine, 3-propylpiperidine, 4-piperidinylpiperidine, (1-cyclopropylpyrrolidone-3-yl)methylamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, N-propylcyclohexylamine, and N,N-dimethylcyclohexylamine.
4. An olefin polymerization reaction system, characterized in that, An anti-sticking agent was added to the olefin polymerization reaction system to allow the anti-sticking agent to come into contact with the catalyst used for olefin polymerization; The anti-sticking agent includes at least one of a nitrogen-containing compound, a sulfur-containing compound, and a phosphorus-containing compound. The nitrogen-containing compound has the general formula of Formula II, the phosphorus-containing compound has the general formula of Formula V or Formula VI, and the sulfur-containing compound is selected from at least one of dipentyl disulfide, 1,9-nonanedithiol, bis(16-hydroxyhexadecyl) disulfide, and dicyclohexyl disulfide. 、 、 Formula II, Formula V, Formula VI in, -R 3 -R 4 -R 5 It is a -H or hydrocarbon group, with a total carbon number between 8 and 60; -R 12 -R 13 -R 14 It is -H, hydrocarbon group or hydrocarbon oxygen group, and the total number of carbons is between 8 and 60.
5. The olefin polymerization reaction system according to claim 4, characterized in that, -R 3 -R 4 -R 5 The total carbon number is between 8 and 30, -R 12 -R 13 -R 14 The total carbon number is between 8 and 30.
6. The olefin polymerization reaction system according to claim 5, characterized in that, The phosphorus-containing compound is selected from at least one of tributyl phosphate, tricyclopentyl phosphate, dibutyl phosphite, 2-ethylhexyl phosphate, tributylphosphine, tricyclohexylphosphine, tri-n-butylphosphine, and trihexylphosphine oxide; the nitrogen-containing compound is selected from at least one of tripentylamine, dihexylamine, dicyclohexylamine, spermine, spermidine, decanediamine, 3-propylpiperidine, 4-piperidinylpiperidine, (1-cyclopropylpyrrolidone-3-yl)methylamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, N-propylcyclohexylamine, and N,N-dimethylcyclohexylamine.
7. A method for olefin polymerization, characterized in that, This olefin polymerization reaction method uses olefins as raw materials, adds an anti-sticking agent and a catalyst for olefin polymerization, and the anti-sticking agent comes into contact with the catalyst for olefin polymerization to carry out the polymerization reaction; The anti-sticking agent includes at least one of a nitrogen-containing compound, a sulfur-containing compound, and a phosphorus-containing compound. The nitrogen-containing compound has the general formula of Formula II, the phosphorus-containing compound has the general formula of Formula V or Formula VI, and the sulfur-containing compound is selected from at least one of dipentyl disulfide, 1,9-nonanedithiol, bis(16-hydroxyhexadecyl) disulfide, and dicyclohexyl disulfide. 、 、 Formula II, Formula V, Formula VI in, -R 3 -R 4 -R 5 It is a -H or hydrocarbon group, with a total carbon number between 8 and 60; -R 12 -R 13 -R 14 It is -H, hydrocarbon group or hydrocarbon oxygen group, and the total number of carbons is between 8 and 60.
8. The olefin polymerization method according to claim 7, characterized in that, The anti-sticking agent is added during the preparation or formulation of the catalyst for olefin polymerization, or the anti-sticking agent and the catalyst for olefin polymerization are added during the olefin prepolymerization process.
9. The olefin polymerization method according to claim 7, characterized in that, The catalyst used for olefin polymerization is a metallocene catalyst, a restricted geometry metallocene catalyst, a non-metallocene catalyst, a supported metallocene catalyst, a supported restricted geometry metallocene catalyst, or a supported non-metallocene catalyst.
10. The olefin polymerization method according to claim 7, characterized in that, The polymerization reaction is a solution polymerization reaction, a gas-phase polymerization reaction, a liquid-phase bulk polymerization reaction, a slurry polymerization reaction, a loop polymerization reaction, or a combination of polymerization reactions.
11. The olefin polymerization method according to claim 7, characterized in that, The olefin polymerization reaction method includes the following steps: Step 1: Ensure that the catalyst for olefin polymerization and the anti-sticking agent are in full contact; Step 2: Mix the co-catalyst with the mixture obtained in Step 1; Step 3: Under the action of the mixture obtained in step 2, the olefin undergoes a polymerization reaction.
12. The olefin polymerization method according to claim 11, characterized in that, The catalyst for olefin polymerization, calculated as a transition metal, has a molar ratio of catalyst to anti-sticking agent of 1:0.01-2, and a molar ratio of catalyst to co-catalyst of 1:10-1000; the co-catalyst is selected from at least one of trimethylaluminum, triethylaluminum, tripropylaluminum, triisobutylaluminum, tri-n-hexylaluminum, tri-tert-butylaluminum, trioctylaluminum, diethylaluminum chloride, diethylaluminum chloride, sesquiethylaluminum chloride, methoxyaluminum, and modified methoxyaluminum.
13. The olefin polymerization method according to claim 11, characterized in that, The polymerization reactions of olefins include ethylene polymerization, propylene polymerization, copolymerization of ethylene with other organic compounds containing carbon-carbon double bonds, and copolymerization of propylene with other organic compounds containing carbon-carbon double bonds, wherein the other organic compounds containing carbon-carbon double bonds are selected from C2-C. 30 α-olefins, C6-C 30 dienes, C3-C 100 Oxygen-containing organic compounds containing carbon double bonds.
14. The olefin polymerization method according to claim 11, characterized in that, The polymerization reaction is carried out at a temperature of 20-200℃, a time of 5-300 min, and a gas pressure of 0.05-40 MPa.
15. The olefin polymerization method according to claim 7, characterized in that, -R 3 -R 4 -R 5 The total carbon number is between 8 and 30, -R 12 -R 13 -R 14 The total carbon number is between 8 and 30.
16. The olefin polymerization method according to claim 7, characterized in that, The phosphorus-containing compound is selected from at least one of tributyl phosphate, tricyclopentyl phosphate, dibutyl phosphite, 2-ethylhexyl phosphate, tributylphosphine, tricyclohexylphosphine, tri-n-butylphosphine, and trihexylphosphine oxide; the nitrogen-containing compound is selected from at least one of tripentylamine, dihexylamine, dicyclohexylamine, spermine, spermidine, decanediamine, 3-propylpiperidine, 4-piperidinylpiperidine, (1-cyclopropylpyrrolidone-3-yl)methylamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, N-propylcyclohexylamine, and N,N-dimethylcyclohexylamine.
17. The olefin polymerization reaction method according to claim 13, characterized in that, The C2-C 30 The α-olefins are selected from ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, dicyclopentadiene, norbornene, or mixtures thereof.
18. The olefin polymerization method according to claim 13, characterized in that, The C3-C 100 The oxygen-containing organic compounds containing carbon-carbon double bonds are selected from 7-octen-1-ol, 9-decen-1-ol, or mixtures thereof.
Citation Information
Patent Citations
Preparation method and application of polyolefin-coated Ziegler-Natta catalyst
CN105542039A
Catalyst for synthesizing high-fluidity polypropylene, preparation method for catalyst and application of catalyst
CN106317268A
Supported catalyst and supporting method and application thereof
CN108727527A
Olefin polymerization process with reduced fouling
US20120046426A1
Ethylene polymerization catalyst, preparation and application thereof
CN101885793A