High-temperature-resistant polyacrylamide for oil displacement and preparation method thereof

By synthesizing high-temperature resistant polyacrylamide with viscosity-reducing, water-blocking, and profile-adjusting functions, the problem of rapid viscosity decrease of polyacrylamide under high temperature and high salinity conditions was solved, thus achieving efficient oil displacement.

CN117624464BActive Publication Date: 2026-11-24SHANDONG JINGXI INFORMATION TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311703820.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-11
Publication Date
2026-11-24
Estimated Expiration
2043-12-11

AI Technical Summary

Technical Problem

Existing polyacrylamide exhibits poor hydrolytic stability and rapid viscosity decrease under high temperature and high salinity conditions, which affects its oil displacement effect.

Method used

A quaternary polymer was synthesized using monomers such as 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, perfluorooctyl ethyl acrylate, and 1-allyl-3-methylimidazolium p-toluenesulfonate. OP-10, K12, starch, and hydroxypropyl methylcellulose were then added to form a high-temperature resistant polyacrylamide for oil displacement with viscosity-reducing, water-blocking, and profile control functions.

Benefits of technology

It improved the viscosity and oil displacement effect of the polymer. The apparent viscosity reached a maximum of 132 mPa·s at a concentration of 0.2 wt%, and the crude oil viscosity reduction rate reached a maximum of 98.9% at 80℃, thus enhancing the oil displacement effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0004602822040000031
    Figure BDA0004602822040000031
  • Figure BDA0004602822040000051
    Figure BDA0004602822040000051
Patent Text Reader

Abstract

The application belongs to the technical field of tertiary oil recovery, and particularly relates to a high-temperature-resistant oil-displacing polyacrylamide and a preparation method thereof. The preparation method is as follows: acrylamide, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, perfluorooctyl ethyl acrylate, 1-allyl-3-methyl imidazole p-toluenesulfonic acid salt, OP-10, K12, starch, hydroxypropyl methyl cellulose, sodium dihydrogen phosphate and deionized water are sequentially added into a reaction kettle, stirring is conducted, pH is adjusted to 7-8, an initiator is added dropwise, stirring reaction is conducted, temperature continues to be raised, temperature-maintaining reaction is conducted, a viscous mixed solution is obtained, temperature is lowered to below 50 DEG C, pH is adjusted to 7-8, the viscous mixed solution is dried and granulated, and the product is obtained. The application has the advantages of simple synthesis process and no by-product; meanwhile, the application has the characteristics of high viscosity and good viscosity reduction effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of tertiary oil recovery technology, specifically relating to a high-temperature resistant polyacrylamide for oil displacement and its preparation method. Background Technology

[0002] With the large-scale exploitation and consumption of conventional oil and gas reservoirs, unconventional oil and gas resources such as tight sandstone gas, coalbed methane, and shale gas, which are characterized by low permeability and ultra-low permeability, and deep, high temperature, urgently need to be developed and utilized. Due to the long-term influence of water drive, the heterogeneity of low-permeability and ultra-low-permeability oil reservoirs has increased, and their porosity and permeability have deteriorated, forming high-permeability channels. Injected water can easily break through along high-permeability layers, resulting in a large amount of water production in oil wells and affecting the oilfield's production capacity.

[0003] To improve oil recovery, polymer flooding and ternary composite flooding technologies are currently being promoted. These technologies involve injecting an aqueous solution of polyacrylamide to improve the oil-water flow ratio, thereby increasing the crude oil content in the produced material.

[0004] Polyacrylamide is a linear water-soluble polymer and one of the most widely used water-soluble polymers. In water, it readily forms hydrogen bonds with water, is easily soluble in water, and exhibits a large hydrodynamic volume after hydration.

[0005] Polyacrylamide is widely used in oilfield production enhancement. However, polyacrylamide is easily hydrolyzed in formation water and is sensitive to some ions in the formation water. As a result, the polymer viscosity drops rapidly. In addition, after strong shearing in the reservoir pores, the polymer molecular chains deform and break, causing the polymer solution viscosity to drop rapidly. The polymer solution will flow along the large pores of the reservoir, reducing the sweep efficiency of the modulating polymer and thus affecting the oil displacement effect.

[0006] CN104448129B discloses a high-temperature resistant hydrolytic copolymer for oilfields, its preparation method, and its application in oil production. It primarily addresses the problem of poor hydrolytic stability of polyacrylamide under high-temperature and high-salinity conditions, a problem present in previous technologies. However, this invention lacks surfactant units in its molecular structure and can only function as a polymer-driven oil recovery agent. Its improved oil recovery principle relies on increasing the oil displacement profile and expanding the swept volume; it does not possess the viscosity-reducing and oil-displacing function of surfactants.

[0007] CN114805677B discloses a polymer flooding agent and its preparation method, relating to the fields of oilfield chemical additives and polymer polymerization. The method includes: reacting a nitrile compound, fuming sulfuric acid, and a long-chain olefin to obtain a dendritic branched monomer; mixing the dendritic branched monomer, acrylamide, acrylic acid, deionized water, and a pH adjuster to obtain a mixed solution; introducing nitrogen gas into the mixed solution, and then adding an initiator to initiate a polymerization reaction to obtain the polymer flooding agent. The polymer flooding agent prepared by this invention has a strong chelating effect on calcium and magnesium ions, making it suitable for operation in high-salinity areas. It exhibits salt resistance, high temperature resistance, and high thermal stability; even after 3 months under anaerobic conditions at 120°C, the solution viscosity still maintains a high retention rate. However, the apparent viscosity of the polymer flooding agent is below 80 mPa·s, resulting in less than ideal water shut-off and profile control effects, thus affecting the oil displacement effect. Summary of the Invention

[0008] This invention addresses the shortcomings of existing technologies by providing a high-temperature resistant polyacrylamide for oil displacement and its preparation method. This invention has the advantages of a simple synthesis process and no byproducts; it also features high viscosity and good viscosity-reducing effect.

[0009] To achieve the above objectives:

[0010] One objective of this invention is to disclose a high-temperature resistant polyacrylamide for oil displacement, the molecular structural formula of which is as follows:

[0011]

[0012] in:

[0013] a = 50000 - 500000;

[0014] b = 10000 - 200000;

[0015] c = 10000 - 200000;

[0016] d = 2000 - 40000.

[0017] Preferably, the viscosity-average molecular weight of the high-temperature resistant polyacrylamide for oil displacement is 20,000,000-30,000,000.

[0018] Another objective of this invention is to disclose a method for preparing the above-mentioned high-temperature resistant polyacrylamide for oil displacement, the specific steps of which are as follows:

[0019] (1) Add acrylamide, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, perfluorooctyl ethyl acrylate, 1-allyl-3-methylimidazolium p-toluenesulfonate, OP-10 (dodecylphenol polyoxyethylene ether), K12 (sodium dodecyl sulfate), starch, hydroxypropyl methylcellulose, sodium dihydrogen phosphate, and deionized water to the reactor in sequence. Purge the reactor and pipelines with nitrogen for 10-20 minutes, stir, and adjust the pH to 7-8 with sodium hydroxide solution.

[0020] (2) Add the initiator dropwise to the reaction vessel. After the addition is complete, stir the reaction until the solution begins to become viscous. Continue the reaction for 10-30 minutes, then continue to heat to 75-80℃ and keep the temperature for 30-60 minutes to obtain a viscous mixture. Cool down to below 50℃ and adjust the pH to 7-8 with sodium hydroxide solution.

[0021] (3) The above viscous mixture is dried and granulated to a particle size of 1-4 mm to obtain the product, high-temperature resistant oil displacement polyacrylamide.

[0022] Preferably, based on 1 mole of acrylamide, the amounts of 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, perfluorooctyl ethyl acrylate, and 1-allyl-3-methylimidazolium p-toluenesulfonate are 0.2-0.4 moles, 0.2-0.4 moles, and 0.04-0.08 moles, respectively.

[0023] Preferably, the weight ratio of OP-10, K12, starch, hydroxypropyl methylcellulose, sodium dihydrogen phosphate, deionized water and acrylamide in step (1) is 0.05-0.1:0.02-0.04:0.05-0.1:0.05-0.1:0.02-0.04:8-12:1.

[0024] Preferably, the initiator in step (2) is a mixed solution of persulfate and sodium bisulfite, with a weight ratio of 0.2-0.5:1 to acrylamide.

[0025] More preferably, the concentration of persulfate is 8-12 wt%, and the concentration of sodium bisulfite is 3-5 wt%.

[0026] More preferably, the persulfate is one of potassium persulfate, ammonium persulfate, and sodium persulfate.

[0027] The reaction equation for the synthesis of the high-temperature resistant polyacrylamide for oil displacement of the present invention is as follows:

[0028]

[0029] The high-temperature resistant polyacrylamide for oil displacement of the present invention is a quaternary polymer with 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, perfluorooctyl ethyl acrylate, and 1-allyl-3-methylimidazolium p-toluenesulfonate as monomers. It has the functions of viscosity reduction, water blocking and profile control, and drag reduction, which can increase the sweep volume of water drive and thus improve the oil displacement effect. Acrylamide is the main polymer component; 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt is an amphoteric surfactant that can reduce the oil-water interfacial tension, decrease crude oil viscosity, and improve the oil displacement effect during oil displacement; perfluorooctyl ethyl acrylate is a typical fluorinated special surfactant that can significantly reduce the interfacial tension between the present invention and crude oil, and its fluorinated lipophilic group can be non-dynamically miscible with crude oil, thus improving the oil displacement effect; 1-allyl-3-methylimidazolium p-toluenesulfonate is an amphoteric surfactant that complements the above surfactant monomers, thereby improving the oil displacement effect. OP-10 and K12 are emulsifiers, and starch and hydroxypropyl methylcellulose are emulsifying and dispersing agents. On the one hand, they can improve the polymerization quality and uniformity, increase the molecular weight of the polymer, and increase the viscosity of the present invention; on the other hand, as surfactants themselves, they can enhance the oil displacement effect.

[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0031] (1) The high-temperature resistant oil displacement polyacrylamide of the present invention has the characteristic of high apparent viscosity, and the apparent viscosity of 0.2wt% concentration can reach up to 132mPa·s.

[0032] (2) The high-temperature resistant oil displacement polyacrylamide of the present invention has a good high-temperature viscosity reduction effect. The viscosity reduction rate of crude oil at 8500 mPa·s can reach up to 98.9% at 80°C with a concentration of 0.2 wt%. Detailed Implementation

[0033] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0034] Example 1

[0035] (1) Add 0.5 mol acrylamide, 0.1 mol 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, 0.2 mol perfluorooctyl ethyl acrylate, 0.02 mol 1-allyl-3-methylimidazolium p-toluenesulfonate, 1.775 g OP-10, 0.88 g K12, 1.775 g starch, 3.24 g hydroxypropyl methylcellulose, 0.71 g sodium dihydrogen phosphate, and 284 g deionized water to the reactor in sequence. Purge the reactor and pipelines with nitrogen for 10 min, stir, and adjust the pH to 7-8 with sodium hydroxide solution.

[0036] (2) Add 7.1g of initiator to the above reaction vessel. The initiator contains 12wt% potassium persulfate and 5wt% sodium bisulfite. After the addition is complete, stir the reaction until the solution begins to become viscous. Continue the reaction for 10min, then continue to heat to 75℃ and keep the reaction at that temperature for 30min to obtain a viscous mixture. Cool down to below 50℃ and adjust the pH to 7-8 with sodium hydroxide solution.

[0037] (3) The above viscous mixture is dried and granulated to a particle size of 1-4 mm to obtain the product, high-temperature resistant oil displacement polyacrylamide.

[0038] Example 2

[0039] (1) Add 0.5 mol acrylamide, 0.12 mol 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, 0.18 mol perfluorooctyl ethyl acrylate, 0.025 mol 1-allyl-3-methylimidazolium p-toluenesulfonate, 1.84 g OP-10, 0.71 g K12, 1.97 g starch, 3.55 g hydroxypropyl methylcellulose, 0.83 g sodium dihydrogen phosphate, and 314 g deionized water to the reactor in sequence. Purge the reactor and pipelines with nitrogen for 20 min, stir, and adjust the pH to 7-8 with sodium hydroxide solution.

[0040] (2) Add 10.3g of initiator to the above reaction vessel. The initiator contains 12wt% potassium persulfate and 4wt% sodium bisulfite. After the addition is complete, stir the reaction until the solution begins to become viscous. Continue the reaction for 20min, then raise the temperature to 80℃ and keep it at that temperature for 60min to obtain a viscous mixture. Cool the temperature to below 50℃ and adjust the pH to 7-8 with sodium hydroxide solution.

[0041] (3) The above viscous mixture is dried and granulated to a particle size of 1-4 mm to obtain the product, high-temperature resistant oil displacement polyacrylamide.

[0042] Example 3

[0043] (1) Add 0.5 mol acrylamide, 0.14 mol 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, 0.16 mol perfluorooctyl ethyl acrylate, 0.03 mol 1-allyl-3-methylimidazolium p-toluenesulfonate, 2.15 g OP-10, 0.96 g K12, 2.78 g starch, 2.64 g hydroxypropyl methylcellulose, 0.99 g sodium dihydrogen phosphate, and 366 g deionized water to the reactor in sequence. Purge the reactor and pipelines with nitrogen for 10 min, stir, and adjust the pH to 7-8 with sodium hydroxide solution.

[0044] (2) Add 17.75g of initiator to the above reaction vessel. The initiator contains 8wt% sodium persulfate and 3wt% sodium bisulfite. After the addition is complete, stir the reaction until the solution begins to become viscous. Continue the reaction for 30min, then raise the temperature to 76℃ and keep it at that temperature for 40min to obtain a viscous mixture. Cool the temperature to below 50℃ and adjust the pH to 7-8 with sodium hydroxide solution.

[0045] (3) The above viscous mixture is dried and granulated to a particle size of 1-4 mm to obtain the product, high-temperature resistant oil displacement polyacrylamide.

[0046] Example 4

[0047] (1) Add 0.5 mol acrylamide, 0.16 mol 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, 0.14 mol perfluorooctyl ethyl acrylate, 0.035 mol 1-allyl-3-methylimidazolium p-toluenesulfonate, 2.89 g OP-10, 1.3 g K12, 3.55 g starch, 1.775 g hydroxypropyl methylcellulose, 1.23 g sodium dihydrogen phosphate, and 426 g deionized water to the reactor in sequence. Purge the reactor and pipelines with nitrogen for 15 min, stir, and adjust the pH to 7-8 with sodium hydroxide solution.

[0048] (2) Add 16.14g of initiator to the above reaction vessel. The initiator contains 8wt% sodium persulfate and 4wt% sodium bisulfite. After the addition is complete, stir the reaction until the solution begins to become viscous. Continue the reaction for 15min, then raise the temperature to 78℃ and keep it at that temperature for 50min to obtain a viscous mixture. Cool the temperature to below 50℃ and adjust the pH to 7-8 with sodium hydroxide solution.

[0049] (3) The above viscous mixture is dried and granulated to a particle size of 1-4 mm to obtain the product, high-temperature resistant oil displacement polyacrylamide.

[0050] Example 5

[0051] (1) Add 0.5 mol acrylamide, 0.18 mol 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, 0.12 mol perfluorooctyl ethyl acrylate, 0.04 mol 1-allyl-3-methylimidazolium p-toluenesulfonate, 3.55 g OP-10, 1.42 g K12, 3.12 g starch, 1.98 g hydroxypropyl methylcellulose, 1.35 g sodium dihydrogen phosphate, and 400 g deionized water to the reactor in sequence. Purge the reactor and pipelines with nitrogen for 12 min, stir, and adjust the pH to 7-8 with sodium hydroxide solution.

[0052] (2) Add 12.3g of initiator to the above reaction vessel. The initiator contains 10wt% ammonium persulfate and 5wt% sodium bisulfite. After the addition is complete, stir the reaction until the solution begins to become viscous. Continue the reaction for 25min, then raise the temperature to 80℃ and keep it at that temperature for 45min to obtain a viscous mixture. Cool the temperature to below 50℃ and adjust the pH to 7-8 with sodium hydroxide solution.

[0053] (3) The above viscous mixture is dried and granulated to a particle size of 1-4 mm to obtain the product, high-temperature resistant oil displacement polyacrylamide.

[0054] Example 6

[0055] (1) Add 0.5 mol acrylamide, 0.2 mol 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, 0.1 mol perfluorooctyl ethyl acrylate, 0.04 mol 1-allyl-3-methylimidazolium p-toluenesulfonate, 3.23 g OP-10, 1.22 g K12, 2.47 g starch, 2.47 g hydroxypropyl methylcellulose, 1.42 g sodium dihydrogen phosphate, and 366 g deionized water to the reactor in sequence. Purge the reactor and pipelines with nitrogen for 18 min, stir, and adjust the pH to 7-8 with sodium hydroxide solution.

[0056] (2) Add 14.2g of initiator to the above reaction vessel. The initiator contains 12wt% ammonium persulfate and 3wt% sodium bisulfite. After the addition is complete, stir the reaction until the solution begins to become viscous. Continue the reaction for 20min, then raise the temperature to 76℃ and keep it at that temperature for 55min to obtain a viscous mixture. Cool the temperature to below 50℃ and adjust the pH to 7-8 with sodium hydroxide solution.

[0057] (3) The above viscous mixture is dried and granulated to a particle size of 1-4 mm to obtain the product, high-temperature resistant oil displacement polyacrylamide.

[0058] Example 7: Apparent viscosity test

[0059] The apparent viscosity of this invention was tested according to method 7.5 in Q / SH1020 1572—2022 "Polyacrylamide for Oil Displacement".

[0060] The oil displacement polyacrylamide from Shengli Chemical Co., Ltd. of Shengli Oilfield was used as a comparative example.

[0061] The test results are shown in Table 1.

[0062] As can be seen from Table 1, the apparent viscosity of the high-temperature resistant oil displacement polyacrylamide of the present invention (Examples 1-6) at a concentration of 0.2 wt% is greater than 115 mPa s, with the highest reaching 132 mPa s; while the apparent viscosity of the comparative example is 88 mPa s, which is significantly lower than that of the present invention.

[0063] Example 8: Determination of viscosity reduction rate

[0064] The high-temperature resistant polyacrylamide for oil displacement of the present invention was prepared into a 0.2 wt% solution and preheated in an 80°C water bath. Crude oil (viscosity 8500 mPa·s) from a heavy oil block in Shengli Oilfield was also preheated in an 80°C water bath. 30g of each solution was placed in a 100ml stoppered graduated cylinder and heated in an 80°C water bath for another 0.5 hours. The stopper was then pressed down and shaken up and down 50-60 times. The viscosity was tested, and the viscosity reduction rate was calculated. The results are shown in Table 1.

[0065]

[0066] In the formula:

[0067] f—viscosity reduction rate, %;

[0068] μ0 — Initial viscosity of crude oil at 80℃, mPa·s;

[0069] μ——Crude oil viscosity after viscosity reduction, mPa·s.

[0070] The oil displacement polyacrylamide from Shengli Chemical Co., Ltd. of Shengli Oilfield was used as a comparative example.

[0071] The test results are shown in Table 1.

[0072] Table 1. Results of Apparent Viscosity and Viscosity Reduction Tests

[0073] Apparent viscosity, mPa·s f,% Example 1 125 98.9 Example 2 128 98.9 Example 3 132 98.8 Example 4 130 98.7 Example 5 118 98.7 Example 6 124 98.6 Comparative Example 88 Non-emulsification

[0074] As can be seen from Table 1, the high-temperature resistant polyacrylamide for oil displacement of the present invention (Examples 1-6) at 0.2 wt% concentration at 80°C has a viscosity reduction rate of more than 98% for crude oil at 8500 mPa·s, with the highest reaching 98.9%; while the oil displacement polyacrylamide of Shengli Chemical Co., Ltd. of Shengli Oilfield in the comparative example does not emulsify.

[0075] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for preparing high-temperature resistant polyacrylamide for oil displacement, characterized in that, The specific steps of the preparation method are as follows: (1) Acrylamide, 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, perfluorooctyl ethyl acrylate, 1-allyl-3-methylimidazolium p-toluenesulfonate, OP-10 (dodecylphenol polyoxyethylene ether), K12 (sodium dodecyl sulfate), starch, hydroxypropyl methylcellulose, sodium dihydrogen phosphate, and deionized water are added sequentially to the reaction vessel. The reaction vessel and pipeline are purged with nitrogen for 10-20 minutes, stirred, and the pH is adjusted to 7-8 with sodium hydroxide solution. The weight ratio of OP-10, K12, starch, hydroxypropyl methylcellulose, sodium dihydrogen phosphate, deionized water and acrylamide is 0.05-0.1:0.02-0.04:0.05-0.1:0.05-0.1:0.02-0.04:8-12:1; (2) Add the initiator dropwise to the above reaction vessel. After the dropwise addition is complete, stir the reaction until the solution begins to become viscous. Continue the reaction for 10-30 minutes, then continue to heat to 75-80℃ and keep the reaction at that temperature for 30-60 minutes to obtain a viscous mixture. Cool down to below 50℃ and adjust the pH to 7-8 with sodium hydroxide solution. The initiator is a mixed solution of persulfate and sodium bisulfite, with a weight ratio of 0.2-0.5:1 to acrylamide. (3) The above viscous mixture is dried and granulated to a particle size of 1-4 mm to obtain the product, high-temperature resistant oil displacement polyacrylamide; Based on 1 mole of acrylamide, the amounts of 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt, perfluorooctyl ethyl acrylate, and 1-allyl-3-methylimidazolium p-toluenesulfonate are 0.2-0.4 moles, 0.2-0.4 moles, and 0.04-0.08 moles, respectively. The molecular structure of the high-temperature resistant polyacrylamide for oil displacement is as follows: in: a=50000-500000; b=10000-200000; c=10000-200000; d=2000-40000。 2. The preparation method of high-temperature resistant polyacrylamide for oil displacement according to claim 1, characterized in that, The concentration of persulfate is 8-12 wt%, and the concentration of sodium bisulfite is 3-5 wt%.

3. The preparation method of a high-temperature resistant polyacrylamide for oil displacement according to claim 2, characterized in that, The persulfate mentioned is one of potassium persulfate, ammonium persulfate, and sodium persulfate.

4. A high-temperature resistant polyacrylamide for oil displacement prepared by the preparation method described in claim 1.

5. The high-temperature resistant polyacrylamide for oil displacement according to claim 4, characterized in that, The viscosity-average molecular weight of the high-temperature resistant polyacrylamide for oil displacement is 20,000,000-30,000,000.

Citation Information

Patent Citations

  • High temperature resistant hydrolysis copolymer for oil field, preparation method and application thereof

    CN104448129B

  • Polymer oil displacement agent solution based on fluorine-containing water-soluble hyperbranched polymer

    CN106117439A

  • Thickening agent for acidizing and fracturing and synthesis method thereof

    CN116751337A