Method for preparing a ternary ethylene propylene rubber anti-swelling nano-coating based on liquid infusion technology
By using liquid infusion technology to prepare a nanoscale anti-swelling coating on the surface of EPDM rubber, the problem of altering the properties of EPDM and the coating thickness affecting sealing performance in existing technologies is solved, achieving the effect of improving anti-swelling performance and applicability without changing the rubber properties.
Patent Information
- Application Number
- CN202311548698.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-20
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-11-20
AI Technical Summary
Existing technologies often alter the bulk properties or affect the surface quality of ethylene propylene diene monomer (EPDM) rubber when improving its anti-swelling properties. Furthermore, the existing coatings are relatively thick, which affects sealing performance and applicability to precision assembly systems.
A nanoscale anti-swelling coating was prepared on the surface of EPDM rubber using liquid infusion technology. The activation sites were increased by oxygen plasma treatment, a fluorinated silane coupling agent was grafted to form a molecular brush, and the coating molecules were fixed by the hydrophobic force of the perfluorinated liquid. The preparation process does not affect the properties of the rubber itself.
Without altering the bulk properties and surface quality of EPDM, solvent diffusion is effectively suppressed, improving the precision assembly applicability of the coating and broadening the application range of EPDM.
Smart Images

Figure HDA0004559014420000011 
Figure HDA0004559014420000012 
Figure HDA0004559014420000013
Abstract
Description
Technical Field
[0001] This invention belongs to the field of nano-coating preparation technology, and relates to a method for preparing an anti-swelling nano-coating for EPDM rubber based on liquid infusion technology. Background Technology
[0002] Ethylene-propylene-diene monomer (EPDM) rubber is a terpolymer made of ethylene, propylene, and non-conjugated dienes. Its molecular backbone is saturated, while the side chains contain a small number of unsaturated double bonds. Commercial production of this rubber material began in 1963, and according to incomplete statistics, global annual consumption of EPDM exceeds 800,000 tons. Compared with other general-purpose rubbers, EPDM has excellent heat resistance, ozone resistance, weather resistance, and electrical insulation properties, and is widely used in sealing mechanical transmission parts, waterproof materials, wires and cables, thermoplastic elastomers, automotive interiors, pipes, and tires. EPDM, when used in combination with other rubbers, can improve the processing performance and physical properties of the compound, reduce costs, and enhance its practicality. EPDM has no polar substituents in its molecular structure, low intermolecular cohesive energy, and low unsaturation. EPDM's unique bulk chemical structure gives its vulcanized products excellent properties in the following aspects: ① EPDM has a low density of 0.87 g / cm³. 3 ① The physical and mechanical properties do not decrease significantly after high filling; ② EPDM molecular chains can maintain flexibility over a wide temperature range (-55~125℃), allowing for short-term or intermittent use within a temperature range of 150~200℃; ③ EPDM has good resistance to various polar chemicals such as alcohols, acids, alkalis, oxidants, refrigerants, ketones, and esters; ④ EPDM has good water vapor resistance, and its surface appearance does not change significantly after being kept in superheated steam at 230℃ for nearly 100 hours.
[0003] Although EPDM exhibits excellent performance in terms of filling properties, aging resistance, and corrosion resistance, its stability in aliphatic and aromatic hydrocarbon solvents (such as gasoline, benzene, and methane) and mineral oils is poor, and it is highly prone to swelling in non-polar hydrocarbon solvents. When EPDM is used as a sealing material in mechanical components such as piston rods, filters, pumps, and valves, the permeation and diffusion of oil and gas media in the mechanical operating system can cause EPDM to swell. This behavior severely affects the sealing performance and surface mechanical properties of EPDM, leading to a series of sealing failure phenomena such as seal ring detachment and structural damage to the sealing material. Therefore, proposing feasible strategies to improve the solvent resistance of EPDM is of great significance for improving its performance and service life.
[0004] Currently, there are two main strategies for improving the anti-swelling properties of EPDM: bulk modification and surface modification. Bulk modification involves adding third-party fillers to the crosslinking system during rubber synthesis to enhance the overall solvent resistance of EPDM. For example, by adding materials such as aramid pulp (see Liu Xiaogang, Li Jinchun, You Xiulan. Journal of Chemical Industry and Engineering (2011)), dicumyl peroxide (see Dai Hongfeng. Journal of Shenyang University of Technology (2018)), paraffin oil (see Darko, CJP Polym. Res. (2022)), and graphene oxide (see Lu, Z., Hu, Y., Zhang, B. et al. J. Polym. Res. (2022)) to the EPDM crosslinking system, the "void" pores inside the EPDM crosslinking network can be filled, adjusting the bulk crosslinking density and thus improving the anti-swelling properties of EPDM. Although bulk modification strategies can effectively improve the solvent resistance of EPDM, doping the polymer crosslinking system with third-party fillers often leads to changes in the physicochemical properties of the rubber material (such as hardness and elastic modulus). At the same time, bulk modification strategies require a long preparation cycle, have high economic costs, and are not suitable for the post-processing modification of commercial EPDM.
[0005] Surface modification strategies involve creating a coating on the outer surface of rubber products without altering the chemical composition and cross-linking structure of the rubber bulk material. This coating inhibits the diffusion of solvent molecules into the rubber, thereby achieving an anti-swelling effect. For example, by preparing glass-like coatings (see Adam RA, Daeyeon L, Thao D. et al. Lab Chip. (2008)), amorphous perfluorinated polymer coatings (see Tianjin Y, Jaebum Choo, Stavros S. et al. Adv. Funct. Mat. (2009)), and titanium oxide coatings (see Albert A, Afke D, J. Ruud VO, et al. Chem. Commun. (2022)), the density of the surface molecular layer can be increased, and the surface free energy of the material can be reduced, thereby improving the solvent resistance of the rubber material. Surface modification strategies allow for the regulation of the anti-swelling properties of rubber without changing the physicochemical properties of the bulk material, making them more suitable for the direct post-processing of commercial rubber products compared to bulk modification strategies. However, the coatings used in current surface modification strategies have a large difference in Poisson's ratio from the bulk material, which alters the surface mechanical properties of the rubber material. In addition, the thickness of such coatings ranges from tens to hundreds of micrometers, resulting in high internal stress and difficulty in controlling coating quality.
[0006] In summary, while existing bulk modification and surface modification strategies provide feasible ways to improve the anti-swelling properties of EPDM, these methods generally have the following shortcomings: ① Bulk modification strategies require the addition of third-party fillers to the crosslinking network of the EPDM bulk, which alters the crosslinking density and mechanical properties of the EPDM bulk, reducing its performance; it also cannot modify already-formed commercial EPDM, making this method relatively unsuitable; ② Surface modification strategies result in thicker coatings, making it difficult to control the surface quality of the coated EPDM material, which can easily affect the sealing performance of parts and their fit with other parts, resulting in poor applicability to precision assembly systems. Therefore, if a method for constructing a nanometer-thick anti-swelling coating based on surface modification can be developed that does not alter the properties of the EPDM bulk or affect its surface quality, it will have a positive impact on broadening the application range of EPDM, improving its performance, and extending its service life. Summary of the Invention
[0007] To address the problems of existing bulk modification methods being unable to modify pre-formed commercial EPDM materials, which can easily alter the properties of EPDM and reduce its performance, and existing surface modification methods resulting in thick coatings that can affect the sealing performance and fit with other parts, this invention provides a method for preparing EPDM anti-swelling nano-coatings based on liquid infusion technology. This method effectively reduces coating thickness without altering the bulk properties or surface quality of EPDM, improves the suitability of coated parts for precision assembly systems, and broadens the applicability of the method to EPDM materials.
[0008] To achieve the above-mentioned objectives, the technical solution adopted by the present invention is as follows:
[0009] A method for preparing an anti-swelling nano-coating for EPDM rubber based on liquid infusion technology includes the following steps:
[0010] (1) Clean and dry EPDM rubber is subjected to oxygen plasma treatment to obtain EPDM rubber substrate;
[0011] (2) Add a fluorinated silane coupling agent or a solution of a fluorinated silane coupling agent into a container, suspend the EPDM rubber substrate in the container to avoid direct contact between the EPDM rubber substrate and the liquid fluorinated silane coupling agent or the solution of the fluorinated silane coupling agent, seal the container and allow it to react fully, graft the fluorinated silane coupling agent onto the surface of the EPDM rubber substrate to form a molecular brush, then remove it, rinse it with acetone and dry it to obtain the grafted EPDM rubber;
[0012] (3) The grafted EPDM rubber is fully immersed in a perfluorinated liquid, so that the perfluorinated liquid molecules are fixed inside the molecular brush by the hydrophobic interaction between the perfluorinated liquid molecules and the fluorinated silane coupling agent. Then it is taken out and dried, thus completing the preparation of the anti-swelling nano-coating on the surface of the EPDM rubber.
[0013] In the above technical solution, the fluorinated silane coupling agent includes at least one of heptadecafluorodecyltrimethoxysilane, heptadecafluorodecyltriethoxysilane, tridecafluorooctyltrimethoxysilane, and tridecafluorooctyltriethoxysilane.
[0014] In step (2) of the above technical solution, it is preferable to calculate per 1mm 2 The ratio of 0.04 to 20 μL of fluorosilane coupling agent or fluorosilane coupling agent solution added to the bottom area of the container is as follows: add fluorosilane coupling agent or fluorosilane coupling agent solution to the container.
[0015] In the above technical solution, the solution of the fluorinated silane coupling agent is formed by dissolving the fluorinated silane coupling agent in an organic solvent. In the fluorinated silane coupling agent solution, the volume ratio of the organic solvent to the fluorinated silane coupling agent does not exceed 1000. For example, in the fluorinated silane coupling agent solution, the volume ratio of the organic solvent to the fluorinated silane coupling agent can be (0.1~1000):1.
[0016] In the above technical solution, the perfluorinated liquid includes a mixture of perfluoroalkanes or a perfluorinated polyether. For example, feasible perfluorinated liquids include 3M Fluorinert oils, such as FC-40, FC-70, etc., and DuPont Krytox oils, such as Krytox 100, Krytox 101, Krytox 103, etc.
[0017] In the above technical solution, in step (2), the container is sealed and the reaction is preferably carried out at 10 to 100°C. In step (3), the temperature when the grafted EPDM rubber is immersed in perfluorinated liquid is preferably controlled to be 10 to 100°C.
[0018] In the above technical solution, the reaction time after sealing the container in step (2) is preferably 0.5 to 48 hours, and the soaking time of the grafted EPDM rubber in the perfluorinated liquid in step (3) is preferably controlled to be 10 minutes to 48 hours.
[0019] In step (1) of the above technical solution, the clean and dry EPDM rubber is obtained by ultrasonically cleaning the EPDM rubber with acetone, ethanol and water in sequence to remove organic contaminants and solid particles from the surface, followed by drying. The drying method used here does not affect the grafting reaction in step (2). Drying methods such as compressed air purging, nitrogen purging or inert gas purging can be used, or drying methods such as baking or natural air drying can be used.
[0020] In step (1) of the above technical solution, when oxygen plasma treatment is used, it is preferable to control the power of oxygen plasma treatment to be 10-1500W and the time to be 10s-10min.
[0021] In step (2) of the above technical solution, the purpose of drying after rinsing with acetone is to remove acetone molecules. The drying method can be compressed air purging, non-reactive gas purging such as nitrogen purging, inert gas purging, drying, and natural air drying.
[0022] In step (3) of the above technical solution, the main purpose of drying the grafted EPDM rubber after fully immersing it in perfluorinated liquid is to remove the perfluorinated liquid that has not been fixed by the molecular brush layer. The drying method is preferably compressed air purging, nitrogen or other non-reactive gas purging, or inert gas purging.
[0023] In the above technical solution, the thickness of the anti-swelling nano-coating prepared on the surface of EPDM rubber is in the nanometer range. The thickness of the anti-swelling nano-coating is usually no more than 1000 nm. The specific thickness can be determined according to the actual application requirements. Furthermore, the thickness of the anti-swelling nano-coating is generally between 100 and 500 nm. For example, the thickness of the anti-swelling nano-coating can be between 150 and 300 nm.
[0024] Compared with the prior art, the technical solution of the present invention can produce the following beneficial technical effects:
[0025] 1. This invention provides a method for preparing an anti-swelling nano-coating for EPDM rubber based on liquid infusion technology. The method first involves treating clean and dry EPDM rubber with oxygen plasma to obtain an EPDM rubber substrate, increasing the activation sites on the EPDM rubber surface, which is beneficial for subsequent grafting reactions. Then, a fluorinated silane coupling agent is grafted onto the surface of the EPDM rubber substrate using chemical vapor deposition to form a uniform molecular brush. Afterwards, the substrate is immersed in a perfluorinated liquid, where the perfluorinated liquid molecules are fixed inside the molecular brush through hydrophobic interactions with the fluorinated silane coupling agent, thus completing the preparation of the anti-swelling nano-coating on the EPDM rubber surface. The method provided by this invention is a surface modification strategy; the preparation process does not affect the properties of the EPDM rubber itself, making it highly suitable for modifying commercially available EPDM rubber materials, with a wide range of applications.
[0026] 2. The anti-swelling coating formed on the surface of EPDM rubber by the method of the present invention has a thickness of nanometers. Compared with the coatings with a thickness of tens to hundreds of micrometers prepared by existing surface modification strategies, the anti-swelling coating with a thickness of nanometers will not affect the sealing performance of the parts or the fit with other parts, and is significantly more suitable for precision assembly systems.
[0027] 3. Experiments have shown that when the thickness of the anti-swelling coating formed on the surface of EPDM rubber is 150-200 nm, it can effectively inhibit the diffusion of aviation hydraulic oil into EPDM rubber, thus playing a good role in inhibiting the swelling of EPDM rubber.
[0028] 4. The method described in this invention has low requirements for instruments, reagents and process conditions. The preparation of anti-swelling nano-coating on the surface of EPDM rubber can be achieved under conventional operating conditions. Therefore, this invention is suitable for promotion and application under existing simple process conditions and is easy to realize industrial production. Attached Figure Description
[0029] Figure 1 This is a schematic flowchart of the method described in this invention. In the figure, 1-EPDM substrate, 2-fluorinated silane coupling agent, 3-fluorinated silane coupling agent molecule, 4-fluorinated silane coupling agent or solution of fluorinated silane coupling agent, 5-container, 6-perfluorinated liquid, 7-grafted EPDM, 8-fluorinated silane coupling agent, 9-perfluorinated liquid molecule.
[0030] Figure 2 This is a scanning electron microscope image of the EPDM surface used in Example 1.
[0031] Figure 3 This is a scanning electron microscope image of the surface of the EPDM prepared in Example 1, which has an anti-swelling nanocoating.
[0032] Figure 4 Figures (a) and (b) show the surface water droplet contact angle test results of blank EPDM and EPDM with anti-swelling nano-coating in Example 1, respectively.
[0033] Figure 5 The results are from the surface elemental analysis of the EPDM used in Example 2.
[0034] Figure 6 The results are the surface elemental analysis results of the EPDM with an anti-swelling nanocoating prepared in Example 2.
[0035] Figure 7 The results are the thickness test results of the EPDM coating with anti-swelling nano-coating prepared in Example 2.
[0036] Figure 8 Figures (a) and (b) show the hexadecane liquid contact angle test results of the blank EPDM and the prepared EPDM with anti-swelling nano-coating in Example 3, respectively.
[0037] Figure 9 This is an optical image of the EPDM used in Example 4.
[0038] Figure 10 This is an optical image of the EPDM with an anti-swelling nanocoating on its surface prepared in Example 4.
[0039] Figure 11 This is an optical image of the EPDM used in Example 5 after swelling.
[0040] Figure 12 This is an optical image of EPDM with an anti-swelling nanocoating on its surface, prepared in Example 5, after swelling.
[0041] Figure 13 The results are the mass change rate test results of EPDM used in Example 6 after swelling for different times.
[0042] Figure 14 The results are the mass change rate test results of EPDM with an anti-swelling nano-coating prepared in Example 6 after swelling for different times.
[0043] Figure 15 The results are the volume change rate test results of EPDM used in Example 7 after swelling for different times.
[0044] Figure 16 The results are the volume change rate test results of EPDM with an anti-swelling nano-coating prepared in Example 7 after swelling for different times. Detailed Implementation
[0045] The following examples further illustrate the method for preparing EPDM rubber anti-swelling nano-coatings based on liquid infusion technology provided by the present invention. It should be noted that the following examples are only for further illustration of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made to the present invention by those skilled in the art based on the above-described content are still within the scope of protection of the present invention.
[0046] In the following embodiments, the ethylene propylene diene monomer (EPDM) rubber and the aviation hydraulic oil used in the rubber swelling experiment were provided by Shenyang Aircraft Industry Group; heptadecyltrimethoxysilane (1H,1H,2H,2H-Perfluorodecyltrimethoxysilane), heptadecyltriethoxysilane, tridecafluorooctyltrimethoxysilane, and tridecafluorooctyltriethoxysilane were purchased from Energy Chemical Company; perfluorinated liquids FC-40 and FC-70 were purchased from Minnesota Mining and Machinery Manufacturing Company (3M); and perfluorinated liquids Krytox 100, Krytox 101, and Krytox 103 were purchased from DuPont.
[0047] A schematic diagram of the process for preparing EPDM anti-swelling nanocoatings based on liquid infusion technology according to the present invention is shown below. Figure 1 As shown, the following is based on Figure 1 The preparation process of the following embodiments is briefly described: Figure 1 As shown in Figure (a), the EPDM substrate (obtained by cleaning, drying, and oxygen plasma treatment) is suspended above the interior of the container (e.g., suspended by a hook above the interior of the container; in the following embodiments, the containers are all flat-bottomed) to avoid direct contact between the EPDM substrate and the liquid fluorosilane coupling agent or solution of fluorosilane coupling agent contained in the container. The container is sealed, and the fluorosilane coupling agent volatilizes and, in molecular form, contacts the surface of the EPDM substrate through vapor deposition and undergoes a grafting reaction to form a molecular brush; as Figure 1 As shown in Figure (b), it will be by Figure 1 In process (a), the grafted EPDM is immersed in a perfluorinated liquid for a period of time. The perfluorinated liquid molecules are fixed inside the molecular brush by hydrophobic interactions with the fluorinated silane coupling agent molecules, resulting in... Figure 1 The anti-swelling nanocoating shown in Figure (c) Figure 1 The part within the dashed box in Figure (c) is a magnified schematic diagram of the anti-swelling nano-coating.
[0048] Example 1
[0049] In this embodiment, a method for preparing an EPDM anti-swelling nanocoating based on liquid infusion technology is provided, and the steps are as follows:
[0050] (1) Use acetone, ethanol and deionized water in sequence to ultrasonically clean EPDM for 240s to remove organic contaminants and solid particles from the EPDM surface. Then use N2 to dry the EPDM surface for later use.
[0051] (2) The EPDM processed in step (1) is placed in a plasma cleaner and treated with oxygen plasma to obtain EPDM substrate. The power of the oxygen plasma treatment is controlled at 50W and the treatment time is 5min.
[0052] (3) Add water to the glass container at 1mm intervals. 2 Add 0.04 μL of heptadecafluorodecyltrimethoxysilane to the bottom area of the container, suspend the EPDM substrate obtained in step (2) in the glass container to avoid direct contact between the EPDM substrate and the liquid heptadecafluorodecyltrimethoxysilane, seal the glass container and react at an ambient temperature of 20-25°C for 12 h, graft heptadecafluorodecyltrimethoxysilane onto the surface of the EPDM substrate to form a molecular brush, then take it out, rinse it with acetone and blow its surface dry with N2 to obtain the grafted EPDM.
[0053] (4) The grafted EPDM obtained in step (3) is immersed in the perfluorinated liquid Krytox 101 at an ambient temperature of 20-25°C for 12 hours. The perfluorinated liquid molecules are fixed inside the molecular brush by the hydrophobic interaction between them and the heptadecafluorodecyltrimethoxysilane molecules, forming a liquid-infused nano-coating on the EPDM surface. Then, the EPDM is removed and blown dry with compressed air to complete the preparation of the anti-swelling nano-coating on the EPDM surface.
[0054] Figure 2 This is a scanning electron microscope image of the surface of the EPDM (blank EPDM) used in this embodiment. Figure 3 This is a scanning electron microscope (SEM) image of the surface of the EPDM with an anti-swelling nanocoating prepared in this embodiment. (Combined with...) Figures 2-3 As can be seen, from a microscopic morphology perspective, the surface of the EPDM prepared in Example 1 with the anti-swelling nano-coating does not show significant changes compared to the surface of blank EPDM.
[0055] The wetting properties of the surface of the blank EPDM used in this embodiment and the surface of the EPDM with the anti-swelling nano-coating prepared in this embodiment were tested using a contact angle meter. The results are as follows: Figure 4 As shown in Figures (a) and (b), by Figure 4It can be seen that the surface of blank EPDM is relatively hydrophilic with a water droplet contact angle of 100.44°, while the surface of EPDM with an anti-swelling nano-coating has a water droplet contact angle of 109.54°, indicating a relatively hydrophobic state. Figure 4 This also demonstrates that this embodiment successfully formed a coating on the surface of blank EPDM.
[0056] Example 2
[0057] This embodiment provides a method for preparing EPDM anti-swelling nanocoatings based on liquid infusion technology. A schematic flowchart of this method is shown below. Figure 1 As shown, the steps are as follows:
[0058] (1) Use acetone, ethanol and deionized water in sequence to ultrasonically clean EPDM for 60s to remove organic contaminants and solid particles on the surface of EPDM. Then use N2 to dry the surface of EPDM for later use.
[0059] (2) The EPDM processed in step (1) is placed in a plasma cleaner and treated with oxygen plasma to obtain EPDM substrate. The power of the oxygen plasma treatment is controlled at 1300W and the treatment time is 10s.
[0060] (3) Add water to the glass container at 1mm intervals. 2 Add 0.04 μL of heptadecafluorodecyltrimethoxysilane solution (heptadecafluorodecyltrimethoxysilane is dissolved in hexane, with a volume ratio of heptadecafluorodecyltrimethoxysilane to hexane of 1:10) to the bottom area of the container. Suspend the EPDM substrate obtained in step (2) in the glass container to avoid direct contact between the EPDM substrate and the liquid heptadecafluorodecyltrimethoxysilane solution. Seal the glass container and place it at an ambient temperature of 20-25°C for 12 hours to form a molecular brush by grafting heptadecafluorodecyltrimethoxysilane onto the surface of the EPDM substrate. Then take it out, rinse it with acetone, and blow its surface dry with N2 to obtain the grafted EPDM.
[0061] (4) The grafted EPDM obtained in step (3) is immersed in perfluorinated liquid FC-40 at an ambient temperature of 20-25°C for 24 hours. The perfluorinated liquid molecules are fixed inside the molecular brush by the hydrophobic interaction between them and heptadecafluorodecyltrimethoxysilane molecules, forming a liquid-infused nano-coating on the EPDM surface. Then, the EPDM is removed and blown dry with compressed air to complete the preparation of the anti-swelling nano-coating on the EPDM surface.
[0062] Figure 5 These are the elemental analysis results of the surface of the EPDM (blank EPDM) used in this embodiment. Figure 6 These are the elemental analysis results of the EPDM surface with an anti-swelling nano-coating prepared in this embodiment. Combined with... Figures 5-6 As can be seen, compared with the surface of blank EPDM, the EPDM with anti-swelling nano-coating prepared in this embodiment has added F element, and the peak value of C element is also significantly increased, indicating that the anti-swelling coating was successfully prepared on the EPDM surface in this embodiment. The coating thickness of the EPDM with anti-swelling nano-coating prepared in this embodiment was measured by ellipsometry. Three test points were randomly selected during the test, and the results showed that the coating thickness was between 155 and 190 nm, indicating that the method of the present invention achieves the preparation of anti-swelling coating with a thickness at the nanometer level.
[0063] Example 3
[0064] This embodiment provides a method for preparing EPDM anti-swelling nanocoatings based on liquid infusion technology. A schematic flowchart of this method is shown below. Figure 1 As shown, the steps are as follows:
[0065] (1) Use acetone, ethanol and deionized water in sequence to ultrasonically clean EPDM for 180s to remove organic contaminants and solid particles from the EPDM surface. Then use N2 to dry the EPDM surface for later use.
[0066] (2) The EPDM processed in step (1) is placed in a plasma cleaner and treated with oxygen plasma to obtain EPDM substrate. The power of the oxygen plasma treatment is controlled at 10W and the treatment time is 10min.
[0067] (3) Add water to the glass container at 1mm intervals. 2 Add 0.04 μL of heptadecafluorodecyltrimethoxysilane solution (heptadecafluorodecyltrimethoxysilane is dissolved in hexane, with a volume ratio of heptadecafluorodecyltrimethoxysilane to hexane of 1:100) to the bottom area of the container. Suspend the EPDM substrate obtained in step (2) in the glass container to avoid direct contact between the EPDM substrate and the liquid heptadecafluorodecyltrimethoxysilane solution. Seal the glass container and place it at an ambient temperature of 20-25°C for 24 hours to form a molecular brush by grafting heptadecafluorodecyltrimethoxysilane onto the surface of the EPDM substrate. Then take it out, rinse it with acetone, and blow its surface dry with N2 to obtain the grafted EPDM.
[0068] (4) The grafted EPDM obtained in step (3) is immersed in perfluorinated liquid FC-70 at an ambient temperature of 20-25°C for 24 hours. The perfluorinated liquid molecules are fixed inside the molecular brush by the hydrophobic interaction between them and heptadecafluorodecyltrimethoxysilane molecules, forming a liquid-infused nano-coating on the EPDM surface. Then, the EPDM is removed and blown dry with compressed air to complete the preparation of the anti-swelling nano-coating on the EPDM surface.
[0069] The contact angle of the EPDM (blank EPDM) surface used in this embodiment and the hexadecane contact angle of the EPDM surface with the anti-swelling nano-coating prepared in this embodiment were characterized using a contact angle measuring instrument. The results are as follows: Figure 8 As shown in Figures (a) and (b), by Figure 8 It can be seen that the hexadecane contact angle of the blank EPDM surface is 70.89°, while the hexadecane contact angle of the EPDM surface with the anti-swelling nano-coating prepared in this embodiment is 43.51°. This indicates that the anti-swelling nano-coating formed on the EPDM surface in this embodiment has a strong ability to repel hexadecane and can effectively inhibit the spread of oily liquids on the coating.
[0070] Example 4
[0071] This embodiment provides a method for preparing EPDM anti-swelling nanocoatings based on liquid infusion technology. A schematic flowchart of this method is shown below. Figure 1 As shown, the steps are as follows:
[0072] (1) Use acetone, ethanol and deionized water in sequence to ultrasonically clean EPDM for 180s to remove organic contaminants and solid particles from the EPDM surface. Then use N2 to dry the EPDM surface for later use.
[0073] (2) The EPDM processed in step (1) is placed in a plasma cleaner and treated with oxygen plasma to obtain EPDM substrate. The power of the oxygen plasma treatment is controlled at 300W and the treatment time is 30s.
[0074] (3) Add water to the glass container at 1mm intervals. 2 Add 0.04 μL of heptadecafluorodecyltrimethoxysilane solution (heptadecafluorodecyltrimethoxysilane is dissolved in heptane, with a volume ratio of heptadecafluorodecyltrimethoxysilane to heptane of 1:100) to the bottom area of the container. Suspend the EPDM substrate obtained in step (2) in the glass container to avoid direct contact between the EPDM substrate and the liquid heptadecafluorodecyltrimethoxysilane solution. Seal the glass container and place it at an ambient temperature of 20-25°C for 6 hours to form a molecular brush by grafting heptadecafluorodecyltrimethoxysilane onto the surface of the EPDM substrate. Then take it out, rinse it with acetone, and blow its surface dry with N2 to obtain the grafted EPDM.
[0075] (4) The grafted EPDM obtained in step (3) is immersed in the perfluorinated liquid Krytox 100 at an ambient temperature of 20-25°C for 18 hours. This allows the perfluorinated liquid molecules to be fixed inside the molecular brush through hydrophobic interactions with heptadecafluorodecyltrimethoxysilane molecules, forming a liquid-infused nano-coating on the EPDM surface. Then, the EPDM is removed and dried by blowing with compressed air, thus completing the preparation of the anti-swelling nano-coating on the EPDM surface.
[0076] Figure 9 This is an optical image of the EPDM (blank EPDM) used in this embodiment. Figure 10 These are optical images of the EPDM with an anti-swelling nanocoating prepared in this embodiment. (Combined with...) Figures 9-10 As can be seen from the macroscopic morphology, the surface of the EPDM prepared in Example 4 with the anti-swelling nano-coating is not significantly different from the surface of the blank EPDM.
[0077] Example 5
[0078] This embodiment provides a method for preparing EPDM anti-swelling nanocoatings based on liquid infusion technology. A schematic flowchart of this method is shown below. Figure 1 As shown, the steps are as follows:
[0079] (1) Use acetone, ethanol and deionized water in sequence to ultrasonically clean the EPDM for 120s to remove organic contaminants and solid particles from the EPDM surface. Then use N2 to dry the EPDM surface for later use.
[0080] (2) The EPDM processed in step (1) is placed in a plasma cleaner and treated with oxygen plasma to obtain EPDM substrate. The power of the oxygen plasma treatment is controlled at 50W and the treatment time is 8min.
[0081] (3) Add water to the glass container at 1mm intervals. 2 Add 0.04 μL of heptadecafluorodecyltrimethoxysilane solution (heptadecafluorodecyltrimethoxysilane is dissolved in heptane, with a volume ratio of heptadecafluorodecyltrimethoxysilane to heptane of 1:1000) to the bottom area of the container. Suspend the EPDM substrate obtained in step (2) in the glass container to avoid direct contact between the EPDM substrate and the liquid heptadecafluorodecyltrimethoxysilane solution. Seal the glass container and place it at an ambient temperature of 20-25°C for 12 hours to form a molecular brush by grafting heptadecafluorodecyltrimethoxysilane onto the surface of the EPDM substrate. Then take it out, rinse it with acetone, and blow its surface dry with N2 to obtain the grafted EPDM.
[0082] (4) The grafted EPDM obtained in step (3) is immersed in the perfluorinated liquid Krytox103 at an ambient temperature of 20-25°C for 6 hours. The perfluorinated liquid molecules are fixed inside the molecular brush by the hydrophobic interaction between them and the heptadecafluorodecyltrimethoxysilane molecules, forming a liquid-infused nano-coating on the EPDM surface. Then, the EPDM is removed and blown dry with compressed air to complete the preparation of the anti-swelling nano-coating on the EPDM surface.
[0083] The EPDM (blank EPDM) used in this embodiment and the EPDM with an anti-swelling nano-coating prepared in this embodiment were completely immersed in aviation hydraulic oil and kept for 4 hours to swell. The two had the same size before swelling. Figure 11 These are optical images of blank EPDM after swelling in this embodiment. Figure 12 These are optical images of the EPDM with an anti-swelling nano-coating prepared in this embodiment after swelling. (Combined with...) Figures 11-12 As can be seen, the EPDM with an anti-swelling nano-coating prepared in this embodiment only showed wrinkles in some surface areas after swelling, but the overall volume of the sample did not change significantly. This is mainly due to the isolation provided by the anti-swelling nano-coating on the EPDM surface, which allowed only a small portion of the solvent to come into contact with the EPDM, resulting in localized swelling. In contrast, the blank EPDM underwent overall deformation and expansion after swelling. This demonstrates that the present invention can effectively suppress the swelling behavior of EPDM by preparing an anti-swelling nano-coating on the EPDM surface.
[0084] Example 6
[0085] This embodiment provides a method for preparing EPDM anti-swelling nanocoatings based on liquid infusion technology. A schematic flowchart of this method is shown below. Figure 1 As shown, the steps are as follows:
[0086] (1) Use acetone, ethanol and deionized water in sequence to ultrasonically clean EPDM for 30s to remove organic contaminants and solid particles on the surface of EPDM. Then use N2 to dry the surface of EPDM for later use.
[0087] (2) The EPDM processed in step (1) is placed in a plasma cleaner and treated with oxygen plasma to obtain EPDM substrate. The power of the oxygen plasma treatment is controlled at 200W and the treatment time is 6min.
[0088] (3) Add water to the glass container at 1mm intervals. 2Add 0.04 μL of heptadecafluorodecyltrimethoxysilane solution (heptadecafluorodecyltrimethoxysilane is dissolved in hexadecane, with a volume ratio of heptadecafluorodecyltrimethoxysilane to hexadecane of 1:10) to the bottom area of the container. Suspend the EPDM substrate obtained in step (2) in the glass container to avoid direct contact between the EPDM substrate and the liquid heptadecafluorodecyltrimethoxysilane solution. Seal the glass container and place it at an ambient temperature of 20-25°C for 18 hours to form a molecular brush by grafting heptadecafluorodecyltrimethoxysilane onto the surface of the EPDM substrate. Then take it out, rinse it with acetone, and blow its surface dry with N2 to obtain the grafted EPDM.
[0089] (4) The grafted EPDM obtained in step (3) is immersed in the perfluorinated liquid Krytox101 at an ambient temperature of 20-25°C for 6 hours. The perfluorinated liquid molecules are fixed inside the molecular brush by the hydrophobic interaction between them and the heptadecafluorodecyltrimethoxysilane molecules, forming a liquid-infused nano-coating on the EPDM surface. Then, the EPDM is removed and blown dry with compressed air to complete the preparation of the anti-swelling nano-coating on the EPDM surface.
[0090] The EPDM (blank EPDM) used in this embodiment and the EPDM with anti-swelling nano-coating prepared in this embodiment were completely immersed in aviation hydraulic oil and kept for 4 hours to swell. During the swelling period, the sample was taken out and dried every 1 hour, and weighed to calculate the mass change rate. The mass change rate (%) = mass of the sample after being taken out and dried after swelling for different times / mass of the sample before swelling × 100%. Figure 13 This is the result of the mass change rate test of blank EPDM after swelling for different times in this embodiment. Figure 14 The mass change rate test results of the EPDM with an anti-swelling nano-coating prepared in this embodiment after swelling for different times. Combined with... Figures 13-14 It can be seen that after 1 hour of swelling, the mass change rate of the EPDM with the anti-swelling nano-coating on the surface prepared in this embodiment is 4%, while the mass change rate of the blank EPDM is 7.7%. With the increase of swelling time, the mass change rate of the blank EPDM increases significantly, while the mass change rate of the EPDM with the anti-swelling nano-coating on the surface is always lower than that of the blank EPDM. After 4 hours of swelling, the mass change rate of the blank EPDM reaches more than 20%, while the mass change rate of the EPDM with the anti-swelling nano-coating on the surface is less than 14%. The above test results show that by preparing an anti-swelling nano-coating on the surface of EPDM, the present invention can effectively inhibit the diffusion of solvent molecules into EPDM, thereby inhibiting the swelling of EPDM rubber.
[0091] Example 7
[0092] This embodiment provides a method for preparing EPDM anti-swelling nanocoatings based on liquid infusion technology. A schematic flowchart of this method is shown below. Figure 1 As shown, the steps are as follows:
[0093] (1) Use acetone, ethanol and deionized water in sequence to ultrasonically clean EPDM for 90s to remove organic contaminants and solid particles on the surface of EPDM. Then use N2 to dry the surface of EPDM for later use.
[0094] (2) The EPDM processed in step (1) is placed in a plasma cleaner and treated with oxygen plasma to obtain EPDM substrate. The power of the oxygen plasma treatment is controlled at 150W and the treatment time is 3min.
[0095] (3) Add water to the glass container at 1mm intervals. 2 Add 0.04 μL of heptadecafluorodecyltrimethoxysilane solution (heptadecafluorodecyltrimethoxysilane is dissolved in hexadecane, with a volume ratio of heptadecafluorodecyltrimethoxysilane to hexadecane of 1:100) to the bottom area of the container. Suspend the EPDM substrate obtained in step (2) in the glass container to avoid direct contact between the EPDM substrate and the liquid heptadecafluorodecyltrimethoxysilane solution. Seal the glass container and place it at an ambient temperature of 20-25°C for 40 h to form a molecular brush by grafting heptadecafluorodecyltrimethoxysilane onto the surface of the EPDM substrate. Then take it out, rinse it with acetone, and blow its surface dry with N2 to obtain the grafted EPDM.
[0096] (4) The grafted EPDM obtained in step (3) is immersed in perfluorinated liquid FC-40 at an ambient temperature of 20-25°C for 40 hours, so that the perfluorinated liquid molecules are fixed inside the molecular brush through the hydrophobic interaction between the perfluorinated liquid molecules and the heptadecafluorodecyltrimethoxysilane molecules, forming a liquid-infused nano-coating on the EPDM surface. Then, it is taken out and blown with compressed air until its surface is dry, thus completing the preparation of the anti-swelling nano-coating on the EPDM surface.
[0097] The EPDM (blank EPDM) used in this embodiment and the EPDM with anti-swelling nano-coating prepared in this embodiment were completely immersed in aviation hydraulic oil and kept for 4 hours to swell. During the swelling period, the sample was taken out and dried every 1 hour, and the volume was measured. The volume change rate was calculated as follows: Volume change rate (%) = Volume of sample after drying after swelling for different times / Volume of sample before swelling × 100%. Figure 15 These are the volume change rate test results of blank EPDM after swelling for different times in this embodiment. Figure 16 This is the test result of the volume change rate of the EPDM with an anti-swelling nano-coating prepared in this embodiment after swelling for different times. Combined with... Figures 15-16It can be seen that, after 1 hour of swelling, the volume change rate of the EPDM with the anti-swelling nano-coating on the surface prepared in this embodiment is no more than 4%, while the volume change rate of the blank EPDM is above 6%. As the swelling time increases, the volume change rate of the blank EPDM increases significantly, while the volume change rate of the EPDM with the anti-swelling nano-coating on the surface is always lower than that of the blank EPDM. After 4 hours of swelling, the volume change rate of the blank EPDM is above 12%, while the volume change rate of the EPDM with the anti-swelling nano-coating on the surface is below 9.5%. The above test results show that by preparing an anti-swelling nano-coating on the surface of EPDM, the present invention can effectively inhibit the diffusion of solvent molecules into EPDM, thereby suppressing the swelling of EPDM rubber.
[0098] Example 8
[0099] This embodiment provides a method for preparing EPDM anti-swelling nanocoatings based on liquid infusion technology. A schematic flowchart of this method is shown below. Figure 1 As shown, the steps are as follows:
[0100] (1) Use acetone, ethanol and deionized water in sequence to ultrasonically clean the EPDM for 120s to remove organic contaminants and solid particles from the EPDM surface. Then use N2 to dry the EPDM surface for later use.
[0101] (2) The EPDM processed in step (1) is placed in a plasma cleaner and treated with oxygen plasma to obtain EPDM substrate. The power of the oxygen plasma treatment is controlled at 300W and the treatment time is 5min.
[0102] (3) Add water to the glass container at 1mm intervals. 2 Add 1 μL of heptadecafluorodecyltriethoxysilane to the bottom area of the container, suspend the EPDM substrate obtained in step (2) in the glass container to avoid direct contact between the EPDM substrate and the liquid heptadecafluorodecyltriethoxysilane, seal the glass container and react at 50-60°C for 1 h, graft heptadecafluorodecyltriethoxysilane onto the surface of the EPDM substrate to form a molecular brush, then take it out, rinse it with acetone and blow its surface dry with N2 to obtain the grafted EPDM.
[0103] (4) The grafted EPDM obtained in step (3) is immersed in the perfluorinated liquid Krytox103 at a temperature of 50-60°C for 1 hour, so that the perfluorinated liquid molecules are fixed inside the molecular brush through the hydrophobic interaction between the perfluorinated liquid molecules and the heptadecafluorodecyltriethoxysilane molecules, forming a liquid-infused nano-coating on the EPDM surface. Then, it is taken out and blown with compressed air until its surface is dry, thus completing the preparation of the anti-swelling nano-coating on the EPDM surface.
[0104] Example 9
[0105] This embodiment provides a method for preparing EPDM anti-swelling nanocoatings based on liquid infusion technology. A schematic flowchart of this method is shown below. Figure 1 As shown, the steps are as follows:
[0106] (1) Use acetone, ethanol and deionized water in sequence to ultrasonically clean the EPDM for 120s to remove organic contaminants and solid particles from the EPDM surface. Then use N2 to dry the EPDM surface for later use.
[0107] (2) The EPDM processed in step (1) is placed in a plasma cleaner and treated with oxygen plasma to obtain EPDM substrate. The power of the oxygen plasma treatment is controlled at 400W and the treatment time is 3min.
[0108] (3) Add water to the glass container at 1mm intervals. 2 Add 20 μL of tridecylfluorooctyltrimethoxysilane solution (obtained by dissolving tridecylfluorooctyltrimethoxysilane in hexadecane, with a volume ratio of tridecylfluorooctyltrimethoxysilane to hexadecane of 1:50) to the bottom area of the container. Suspend the EPDM substrate obtained in step (2) in the glass container to avoid direct contact between the EPDM substrate and the liquid tridecylfluorooctyltrimethoxysilane solution. Seal the glass container and place it at a temperature of 90-100°C for 0.5 h to graft tridecylfluorooctyltrimethoxysilane onto the surface of the EPDM substrate to form a molecular brush. Then remove it, rinse it with acetone, and blow its surface dry with N2 to obtain the grafted EPDM.
[0109] (4) Immerse the grafted EPDM obtained in step (3) in the perfluorinated liquid Krytox101 at an ambient temperature of 90-100℃ for 10 minutes. This allows the perfluorinated liquid molecules to be fixed inside the molecular brush through hydrophobic interactions with the molecules of tridecylfluorooctyltrimethoxysilane, forming a liquid-infused nano-coating on the EPDM surface. Then, remove the EPDM and blow it dry with compressed air to complete the preparation of the anti-swelling nano-coating on the EPDM surface.
[0110] Example 10
[0111] This embodiment provides a method for preparing EPDM anti-swelling nanocoatings based on liquid infusion technology. A schematic flowchart of this method is shown below. Figure 1 As shown, the steps are as follows:
[0112] (1) Use acetone, ethanol and deionized water in sequence to ultrasonically clean the EPDM for 120s to remove organic contaminants and solid particles from the EPDM surface. Then use N2 to dry the EPDM surface for later use.
[0113] (2) The EPDM processed in step (1) is placed in a plasma cleaner and treated with oxygen plasma to obtain EPDM substrate. The power of the oxygen plasma treatment is controlled to be 1000W and the treatment time is 30s.
[0114] (3) Add water to the glass container at 1mm intervals. 2 Add 5 μL of tridecylfluorooctyltriethoxysilane solution (obtained by dissolving tridecylfluorooctyltriethoxysilane in heptane, with a volume ratio of tridecylfluorooctyltriethoxysilane to heptane of 1:10) to the bottom area of the container. Suspend the EPDM substrate obtained in step (2) in the glass container to avoid direct contact between the EPDM substrate and the liquid tridecylfluorooctyltriethoxysilane solution. Seal the glass container and place it at an ambient temperature of 10-20°C for 48 hours to form a molecular brush by grafting tridecylfluorooctyltriethoxysilane onto the surface of the EPDM substrate. Then remove it, rinse it with acetone, and dry its surface with N2 to obtain the grafted EPDM.
[0115] (4) The grafted EPDM obtained in step (3) is immersed in the perfluorinated liquid Krytox 100 at an ambient temperature of 10-20°C for 48 hours, so that the perfluorinated liquid molecules are fixed inside the molecular brush through the hydrophobic interaction between the perfluorinated liquid molecules and the tridecylfluorooctyltriethoxysilane molecules, forming a liquid-infused nano-coating on the EPDM surface. Then, it is taken out and blown with compressed air until its surface is dry, thus completing the preparation of the anti-swelling nano-coating on the EPDM surface.
Claims
1. A method for preparing an anti-swelling nano-coating for EPDM rubber based on liquid infusion technology, characterized in that, Includes the following steps: (1) Clean and dry EPDM rubber is subjected to oxygen plasma treatment to obtain EPDM rubber substrate; (2) Add a fluorinated silane coupling agent or a solution of a fluorinated silane coupling agent into a container, suspend the EPDM rubber substrate in the container to avoid direct contact between the EPDM rubber substrate and the liquid fluorinated silane coupling agent or the solution of the fluorinated silane coupling agent, seal the container and allow it to react fully, graft the fluorinated silane coupling agent onto the surface of the EPDM rubber substrate to form a molecular brush, then remove it, rinse it with acetone and dry it to obtain the grafted EPDM rubber; (3) The grafted EPDM rubber is fully immersed in a perfluorinated liquid, so that the perfluorinated liquid molecules are fixed inside the molecular brush by the hydrophobic interaction between the perfluorinated liquid molecules and the fluorinated silane coupling agent. Then it is taken out and dried, thus completing the preparation of the anti-swelling nano-coating on the surface of the EPDM rubber.
2. The method for preparing an anti-swelling nano-coating of EPDM rubber based on liquid infusion technology according to claim 1, characterized in that, The fluorinated silane coupling agent includes at least one of heptadecafluorodecyltrimethoxysilane, heptadecafluorodecyltriethoxysilane, tridecafluorooctyltrimethoxysilane, and tridecafluorooctyltriethoxysilane.
3. The method for preparing an anti-swelling nano-coating of EPDM rubber based on liquid infusion technology according to claim 1, characterized in that, In step (2), according to every 1mm 2 The ratio of 0.04 to 20 μL of fluorosilane coupling agent or fluorosilane coupling agent solution added to the bottom area of the container is as follows: add fluorosilane coupling agent or fluorosilane coupling agent solution to the container.
4. The method for preparing an anti-swelling nano-coating of EPDM rubber based on liquid infusion technology according to claim 1, characterized in that, The solution of the fluorinated silane coupling agent is formed by dissolving the fluorinated silane coupling agent in an organic solvent, wherein the volume ratio of the organic solvent to the fluorinated silane coupling agent in the solution does not exceed 1000.
5. The method for preparing an anti-swelling nano-coating of EPDM rubber based on liquid infusion technology according to claim 1, characterized in that, The perfluorinated liquid includes mixtures of perfluoroalkanes or perfluoropolyethers.
6. The method for preparing an anti-swelling nano-coating of EPDM rubber based on liquid infusion technology according to any one of claims 1 to 5, characterized in that, In step (2), the container is sealed and the reaction is carried out at 10-100°C. In step (3), the temperature of the grafted EPDM rubber is controlled to be 10-100°C when it is immersed in perfluorinated liquid.
7. The method for preparing an anti-swelling nano-coating of EPDM rubber based on liquid infusion technology according to any one of claims 1 to 5, characterized in that, In step (2), the container is sealed and reacted for 0.5–48 hours.
8. The method for preparing an anti-swelling nano-coating for EPDM rubber based on liquid infusion technology according to any one of claims 1 to 5, characterized in that, In step (3), the soaking time of the grafted EPDM rubber in the perfluorinated liquid is controlled to be 10 min to 48 h.
9. The method for preparing an anti-swelling nano-coating for EPDM rubber based on liquid infusion technology according to any one of claims 1 to 5, characterized in that, The clean and dry EPDM rubber mentioned in step (1) is obtained by ultrasonically cleaning the EPDM rubber with acetone, ethanol and water in sequence to remove organic contaminants and solid particles from the surface, followed by drying.
10. The method for preparing an anti-swelling nano-coating of EPDM rubber based on liquid infusion technology according to any one of claims 1 to 5, characterized in that, In step (1), the power of oxygen plasma treatment is controlled to be 10-1500W and the time is 10s-10min.
Citation Information
Patent Citations
Rain-attenuation-proof radome with microporous structure and preparation method thereof
CN108864624A
Surface modification process
US20040071906A1