Resin composition, and prepreg, metal foil laminate, and printed wiring board produced using the same

By adding bismaleimide resin and flame retardants with specific structures to epoxy resin, the resulting resin composition improves the adhesion and dielectric properties of printed circuit boards, solves the thermal stability and environmental protection problems existing in the prior art, and achieves better electrical properties and processing performance.

CN117624837BActive Publication Date: 2026-11-24TAIWAN UNION TECHNOLOGY CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211078755.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-08-18
Filing Date
2022-09-05
Publication Date
2026-11-24
Estimated Expiration
2042-09-05

AI Technical Summary

Technical Problem

Existing epoxy resin-based printed circuit boards, after adding bismaleimide resin, suffer from problems such as insufficient adhesion between dielectric materials and metal foil, poor dielectric properties, and insufficient thermal stability. Furthermore, the use of halogenated flame retardants is subject to environmental restrictions.

Method used

A resin composition is formed by using a combination of epoxy resin, bismaleimide resin and flame retardant with a specific structure, and by adjusting its weight ratio and adding other components such as hardeners and fillers, to improve adhesion, dielectric properties and thermal stability.

Benefits of technology

It improves the glass transition temperature, coefficient of thermal expansion, heat resistance, electrical properties, electrical properties after moisture absorption, dimensional stability, and adhesion of the metal layer of printed circuit boards, and improves processability, solving the problem of dielectric degradation caused by bismaleimide resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117624837B_ABST
    Figure CN117624837B_ABST
Patent Text Reader

Abstract

The present application provides a resin composition and applications thereof. The resin composition comprises: (A) an epoxy resin; (B) a bismaleimide resin; and (C) a first flame retardant having the following formula (I): wherein Ar, R1, R2 and R3 are defined in the specification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a resin composition, and more particularly to an epoxy resin composition containing a specific flame retardant. The resin composition of this invention can be used with reinforcing materials to form a prepreg, or as an adhesive for metal foils, to prepare metal-clad laminates and printed circuit boards (PCBs). Background Technology

[0002] Printed circuit boards (PCBs) are the circuit boards of electronic devices. They mount other electronic components and electrically connect them to provide a stable circuit operating environment. A common PCB substrate is the copper clad laminate (CCL), which is mainly composed of resin, reinforcing materials, and copper foil. Common resins include epoxy resin, phenolic resin, polyurethane, silicone, and Teflon; commonly used reinforcing materials include fiberglass cloth, fiberglass mat, insulating paper, and linen.

[0003] Generally, printed circuit boards (PCBs) can be manufactured as follows: A reinforcing material, such as glass fabric, is impregnated in a resin composition (e.g., an epoxy resin composition), and the glass fabric impregnated with the resin composition is cured to a semi-cured state (i.e., B-stage) to obtain a semi-cured sheet. Subsequently, a predetermined number of semi-cured sheets are stacked, and a metal foil is stacked on at least one outer side of the stacked semi-cured sheets to provide a laminate. The laminate is then subjected to a hot-pressing operation (i.e., C-stage) to obtain a metal foil laminate. The metal foil on the surface of the metal foil laminate is etched to form a specific circuit pattern. Then, multiple holes are drilled in the metal foil laminate, and conductive material is plated into these holes to form via holes, thereby completing the fabrication of the PCB.

[0004] When using epoxy resin compositions to manufacture printed circuit boards (PCBs), various flame retardants, such as halogenated or phosphorus-containing flame retardants, are typically added to impart flame retardancy to the electronic materials. However, the use of halogenated flame retardants has been restricted due to environmental concerns. Commonly used phosphorus-containing flame retardants include phosphazene compounds (such as SPB-100 produced by Otsuka Chemicals) or condensed phosphate esters (such as PX-200 produced by Daihachi Chemicals). However, these flame retardants suffer from problems such as low melting points, low thermal decomposition temperatures, and excessively high high-temperature ionization. Consequently, the resulting substrates have a high coefficient of thermal expansion, making them prone to internal layer cracking during PCB manufacturing, thus reducing process quality.

[0005] WO2010 / 135398 discloses a phosphorus-containing flame retardant, which is a derivative of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO). This derivative has a molecule center containing two DOPO groups (DiDOPO) and has good thermal stability and flame retardancy.

[0006] Furthermore, it is known that bismaleimide (BMI) resin can be used as an alternative to epoxy resin, or added to epoxy resin compositions to improve the heat resistance of the resulting dielectric material. However, adding bismaleimide resin results in poor adhesion of the dielectric material to metal foils (e.g., poor tear strength) and poor dielectric properties (e.g., dissipation factor (Df)). These drawbacks have limited the application of bismaleimide resin in epoxy resin systems.

[0007] Therefore, there is an urgent need in the field to develop a new resin composition to solve the above problems. Summary of the Invention

[0008] The inventors have discovered that the aforementioned technical problems can be unexpectedly solved by using bismaleimide resin and a flame retardant with a specific structure in epoxy resin compositions. Electronic materials made from these epoxy resin compositions can possess excellent glass transition temperature (Tg), coefficient of thermal expansion (z-CTE), heat resistance, electrical properties, electrical properties after moisture absorption, dimensional stability, adhesion to metal layers (tear strength), flame retardancy, and processability (such as warpage and filler properties). Furthermore, the degradation in tear strength and electrical properties caused by the use of bismaleimide resin in epoxy resin systems can also be improved.

[0009] Therefore, one object of the present invention is to provide a resin composition comprising:

[0010] (A) Epoxy resin;

[0011] (B) Bismaleimide resin; and

[0012] (C) The first flame retardant, having the structure of formula (I):

[0013] Formula (I),

[0014] in,

[0015] Ar is C3 to C 18 heteroaryl or C6 to C 18 Aryl;

[0016] R1 is hydrogen or C1 to C2. 18 Alkyl groups; and

[0017] R2 and R3 are each independently hydrogen, C1 to C3. 18 Alkyl, C3 to C 18 heteroaryl, or C6 to C 18 Aryl.

[0018] In some embodiments of the present invention, the weight ratio of the bismaleimide resin (B) to the first flame retardant (C) is 5:1 to 1:5.

[0019] In some embodiments of the present invention, the epoxy resin (A) is selected from the group consisting of: bisphenol type epoxy resins, phenolic type epoxy resins, stilbene type epoxy resins, epoxy resins containing a triazine backbone, epoxy resins containing a pyridine backbone, pyromethane type epoxy resins, xylylene type epoxy resins, biphenyl type epoxy resins, biphenyl aralkyl type epoxy resins, naphthalene type epoxy resins, dicyclopentadiene (DCPD) type epoxy resins, alicyclic epoxy resins, and combinations thereof.

[0020] In some embodiments of the present invention, the bismaleimide resin (B) has a structure represented by the following formula (II):

[0021] Equation (II),

[0022] R4 is selected from the following groups: -CH2- , , , , , ,and , Represents the connection site.

[0023] In some embodiments of the present invention, the bismaleimide resin (B) is selected from the group consisting of: 1,2-bismaleimide ethane, 1,6-bismaleimide hexane, 1,3-bismaleimide benzene, 1,4-bismaleimide benzene, 2,4-bismaleimide toluene, 4,4'-bismaleimide diphenylmethane, 4,4'-bismaleimide diphenyl ether, 3,3'-bismaleimide diphenyl sulfone, 4,4'-bismaleimide diphenyl ether. Phenyl sulfone, 4,4'-bismaleimide dicyclohexylmethane, 3,5-bis(4-maleimide phenyl)pyridine, 2,6-bismaleimide pyridine, 1,3-bis(maleimide methyl)cyclohexane, 1,3-bis(maleimide methyl)benzene, 1,1-bis(4-maleimide phenyl)cyclohexane, 1,3-bis(dichloromaleimide)benzene, 4,4'-biscitraconiimide diphenylmethane (4,4'-biscitraconi midodiphenylmethane), 2,2-bis(4-maleiminophenyl)propane, 1-phenyl-1,1-bis(4-maleiminophenyl)ethane, α,α-bis(4-maleiminophenyl)toluene, 3,5-bismaleimino-1,2,4-triazole, N,N'-epenylethylbismaleimide, N,N'-hexamethylenebismaleimide, N,N'-m-epenylphenylbismaleimide, N,N'-p-epenylphenylbismaleimide Maleimide, N,N'-4,4'-diphenylmethane bismaleimide, N,N'-4,4'-diphenyl ether bismaleimide, N,N'-4,4'-diphenyl sulfone bismaleimide, N,N'-4,4'-dicyclohexylmethane bismaleimide, N,N'-α,α'-4,4'-dimethylenecyclohexane bismaleimide, N,N'-m-xylene bismaleimide, N,N'-4,4'-diphenylcyclohexane bismaleimide, and combinations thereof.

[0024] In some embodiments of the present invention, the first flame retardant (C) is selected from the group consisting of:

[0025] Formula (I-1),

[0026] Formula (I-2),

[0027] Formula (I-3),

[0028] Formula (I-4),

[0029] Formula (I-5),

[0030] Formula (I-6) and its combinations.

[0031] In some embodiments of the present invention, the contents of the bismaleimide resin (B) and the first flame retardant (C) are each independently 5% to 35% by weight, based on the solid content of the resin composition.

[0032] In some embodiments of the present invention, the content of the epoxy resin (A) is 3% to 15% by weight, based on the solid content of the resin composition.

[0033] In some embodiments of the present invention, the resin composition further comprises a curing agent selected from the group consisting of cyanate ester resins, benzoxazine resins, phenol novolac (PN), styrene maleic anhydride (SMA) resins, dicyandiamide (Dicy), diaminodiphenyl sulfone (DDS), amino triazinenovolac (ATN) resins, diaminodiphenylmethane, styrene-vinylphenol copolymers, and combinations thereof.

[0034] In some embodiments of the present invention, the resin composition further comprises a curing accelerator selected from the group consisting of imidazole compounds, pyridine compounds, and combinations thereof.

[0035] In some embodiments of the present invention, the resin composition further comprises fillers selected from the group consisting of: silica (including hollow silica), alumina, magnesium oxide, magnesium hydroxide, calcium carbonate, talc, clay, aluminum nitride, boron nitride, aluminum hydroxide, silicon aluminum carbide, silicon carbide, sodium carbonate, titanium dioxide, zinc oxide, zirconium oxide, quartz, diamond, diamond-like material, graphite, calcined kaolin, baiji, mica, hydrotalcite, polytetrafluoroethylene (PTFE) powder, glass beads, ceramic whiskers, carbon nanotubes, nano-scale inorganic powders, and combinations thereof.

[0036] Another object of the present invention is to provide a semi-cured sheet, which is obtained by impregnating or coating a substrate with the above-mentioned resin composition and drying the impregnated or coated substrate.

[0037] Another object of the present invention is to provide a metal foil laminate, which is obtained by laminating the above-mentioned prepreg with a metal foil, or by coating the above-mentioned resin composition onto a metal foil and drying the coated metal foil.

[0038] Another object of the present invention is to provide a printed circuit board made of the above-mentioned metal foil laminate. Detailed Implementation

[0039] The following describes some specific embodiments of the present invention; however, the present invention can be practiced in many different forms and should not be construed as limited to the description herein.

[0040] Unless otherwise stated, the terms “a,” “the,” and similar terms used in this specification and the claims of the patent application shall be understood to include both singular and plural forms.

[0041] Unless otherwise stated, when describing the components contained in solutions, mixtures, compositions or adhesives in this specification and the claims, the content is calculated as dry weight, that is, the weight excluding solvent.

[0042] Unless otherwise stated, the terms “first,” “second,” and similar terms used in this specification and the claims are used only to distinguish the described elements or components and have no special meaning in themselves, and are not intended to represent a sequence.

[0043] The resin composition of this invention, through the combined use of epoxy resin, bismaleimide resin, and a flame retardant with a specific structure, enables the resulting electronic materials to possess excellent glass transition temperature, coefficient of thermal expansion, heat resistance, electrical properties, electrical properties after moisture absorption, dimensional stability, adhesion to metal layers (tear strength), flame retardancy, and processability (such as warpage and filler properties). Simultaneously, it can improve the tear strength and electrical property degradation caused by the use of bismaleimide resin in epoxy resin systems. The following provides a detailed description of the resin composition of this invention and its related applications.

[0044] 1. Resin composition

[0045] The resin composition of this invention comprises (A) epoxy resin, (B) bismaleimide resin and (C) a first flame retardant having a specific structure as essential components, and may further include optional components as needed. Detailed descriptions of each component are as follows.

[0046] 1.1. (A) Epoxy resin

[0047] In this document, epoxy resin refers to a thermosetting resin having at least two epoxy functional groups in one molecule, such as polyfunctional epoxy resins, phenolic epoxy resins, or combinations thereof. Examples of polyfunctional epoxy resins include, but are not limited to, difunctional epoxy resins, tetrafunctional epoxy resins, and octafunctional epoxy resins. There are no particular limitations on the type of epoxy resin, and those skilled in the art can select one as needed after reviewing this specification. For example, bromine-containing epoxy resins can be used to impart better flame-retardant properties to thermosetting resin compositions, and halogen-free (such as bromine) epoxy resins can also be used to meet halogen-free environmental requirements.

[0048] Epoxy resins that can be used in this invention include, but are not limited to, bisphenol-type epoxy resins, phenolic-type epoxy resins, stilbene-type epoxy resins, epoxy resins containing a triazine backbone, epoxy resins containing a pyridine backbone, triphenol-methane-type epoxy resins, xylylene-type epoxy resins, biphenyl-type epoxy resins, biphenyl aralkyl-type epoxy resins, naphthalene-type epoxy resins, dicyclopentadiene (DCPD)-type epoxy resins, and alicyclic epoxy resins. Examples of bisphenol-type epoxy resins include, but are not limited to, bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, and bisphenol S-type epoxy resins. Examples of phenolic-type epoxy resins (e.g., linear phenolic epoxy resins) include, but are not limited to, phenolic-phenolic-type epoxy resins, cresol-phenolic-phenolic-type epoxy resins, bisphenol A-phenolic-phenolic-type epoxy resins, and bisphenol F-phenolic-phenolic-type epoxy resins. Examples of epoxy resins may also include diglycidyl ether compounds of polyfunctional phenols and polycyclic aromatic compounds such as anthracene.

[0049] The aforementioned epoxy resins can be used individually or in combination, and those skilled in the art can formulate them according to actual needs. In some embodiments of the present invention, bisphenol A type epoxy resin, phenolic type epoxy resin, or a combination thereof are used.

[0050] Generally, based on the solid content of the resin composition, the content of epoxy resin can be from 3% to 15% by weight, for example, 3% by weight, 3.5% by weight, 4% by weight, 4.5% by weight, 5% by weight, 5.5% by weight, 6% by weight, 6.5% by weight, 7% by weight, 7.5% by weight, 8% by weight, 8.5% by weight, 9% by weight, 9.5% by weight, 10% by weight, 10.5% by weight, 11% by weight, 11.5% by weight, 12% by weight, 12.5% ​​by weight, 13% by weight, 13.5% by weight, 14% by weight, 14.5% by weight, or 15% by weight, or within the range of any two of the above values, but the present invention is not limited thereto.

[0051] 1.2. (B) Bismaleimide resin

[0052] In this article, bismaleimide resin refers to a compound or polymer having two maleimide functional groups. Bismaleimide resins possess maleimide functional groups containing reactive double bonds, allowing them to undergo crosslinking reactions with other components containing unsaturated functional groups or epoxy groups. When a resin composition includes bismaleimide resin, the heat resistance of the resulting electronic materials can be improved.

[0053] The bismaleimide resin of the present invention may have a structure represented by the following formula (II):

[0054] Equation (II),

[0055] In equation (II), R4 is selected from the following group: -CH2- , , , , , ,and , Represents the connection site.

[0056] Specific examples of bismaleimide resins include, but are not limited to: 1,2-bismaleimide ethane, 1,6-bismaleimide hexane, 1,3-bismaleimide benzene, 1,4-bismaleimide benzene, 2,4-bismaleimide toluene, 4,4'-bismaleimide diphenylmethane, 4,4'-bismaleimide diphenyl ether, 3,3'-bismaleimide diphenyl sulfone, 4,4'-bismaleimide diphenyl sulfone, and 4,4'-bismaleimide. 3,5-bis(4-maleimide-phenyl)pyridine, 2,6-bismaleimide-pyridine, 1,3-bis(maleimide-methyl)cyclohexane, 1,3-bis(maleimide-methyl)benzene, 1,1-bis(4-maleimide-phenyl)cyclohexane, 1,3-bis(dichloromaleimide-phenyl)benzene, 4,4'-biscitraconimidodiphenylmethane e), 2,2-bis(4-maleimide-phenyl)propane, 1-phenyl-1,1-bis(4-maleimide-phenyl)ethane, α,α-bis(4-maleimide-phenyl)toluene, 3,5-bismaleimide-1,2,4-triazole, N,N'-epenylethylbismaleimide, N,N'-hexamethylenebismaleimide, N,N'-m-epenylphenylbismaleimide, N,N'-p-epenylphenylbismaleimide, N,N'-4,4'-diphenylmethyl Alkyl bismaleimide, N,N'-4,4'-diphenyl ether bismaleimide, N,N'-4,4'-diphenyl sulfone bismaleimide, N,N'-4,4'-dicyclohexylmethane bismaleimide, N,N'-α,α'-4,4'-dimethylenecyclohexane bismaleimide, N,N'-m-xylene bismaleimide, N,N'-4,4'-diphenylcyclohexane bismaleimide, and N,N'-methylenebis(3-chloro-p-ephthyl)bismaleimide. Commercially available bismaleimide resins include products of type BMI-70 and BMI-80 available from KI Chemical, and products of type BMI-1000, BMI-2300, BMI-4000, BMI-5000, BMI-5100, and BMI-7000 available from Daiwa Chemical Industries.

[0057] The aforementioned bismaleimide resins can be used alone or in combination, and those skilled in the art can formulate them according to actual needs. In some embodiments of the present invention, 4,4'-diphenylmethane bismaleimide is used (i.e., the scheme in which R4 of formula (II) is 4,4'-diphenylmethane).

[0058] Generally, based on the solid content of the resin composition, the content of bismaleimide resin (B) can range from 5% to 35% by weight, for example, 5% by weight, 5.5% by weight, 6% by weight, 6.5% by weight, 7% by weight, 7.5% by weight, 8% by weight, 8.5% by weight, 9% by weight, 9.5% by weight, 10% by weight, 10.5% by weight, 11% by weight, 11.5% by weight, 12% by weight, 12.5% ​​by weight, 13% by weight, 13.5% by weight, 14% by weight, 14.5% by weight, 15% by weight, 15.5% by weight, 16% by weight, 16.5% by weight, 17% by weight, 17.5% by weight, 18% by weight, 18.5% by weight, 19% by weight, 19.5% by weight. %, 20% by weight, 20.5% by weight, 21% by weight, 21.5% by weight, 22% by weight, 22.5% by weight, 23% by weight, 23.5% by weight, 24% by weight, 24.5% by weight, 25% by weight, 25.5% by weight, 26% by weight, 26.5% by weight, 27% by weight, 27.5% by weight, 28% by weight, 28.5% by weight, 29% by weight, 29.5% by weight, 30% by weight, 30.5% by weight, 31% by weight, 31.5% by weight, 32% by weight, 32.5% by weight, 33% by weight, 33.5% by weight, 34% by weight, 34.5% by weight, or 35% by weight, or a range consisting of any two of the above values, but the present invention is not limited thereto.

[0059] 1.3. (C) First flame retardant

[0060] Generally, flame retardants can improve the flame retardancy of electronic materials. In this paper, the first flame retardant is a compound having a specific structure of formula (I):

[0061] Formula (I),

[0062] In equation (I), Ar can be C3 to C 18 heteroaryl or C6 to C 18 Aryl; R1 can be hydrogen or C1 to C1. 18 Alkyl groups; and R2 and R3 may each be independently hydrogen, C1 to C3. 18 Alkyl, C3 to C 18 heteroaryl, or C6 to C 18 Aryl. The above C3 to C 18 Heteroaryl refers to an aromatic ring or fused ring structure having 3 to 18 carbon atoms, containing one or more heteroatoms (such as oxygen, nitrogen, and sulfur) in one or more aromatic rings or fused rings. The above C6 to C... 18 The aryl group refers to aromatic monocyclic, polycyclic, or fused-ring structures having 6 to 18 carbon atoms. (C3 to C4) 18 Examples of heteroaryl groups include, but are not limited to, pyridyl, furanyl, and imidazole; C6 to C6.18 Examples of aryl groups include, but are not limited to, phenyl, naphthyl, and anthracene; and C1 to C2 groups. 18 Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, and isobutyl. Furthermore, the Ar group of the first flame retardant is preferably phenyl, naphthyl, or anthracene, more preferably phenyl or naphthyl, and especially preferably phenyl. When the first flame retardant meets the above conditions, the electronic material made from the resin composition can have better properties, including better thermal expansion and electrical properties after moisture absorption.

[0063] Examples of the first flame retardant (C) include, but are not limited to, at least one selected from the following groups:

[0064] Formula (I-1),

[0065] Formula (I-2),

[0066] Formula (I-3),

[0067] Formula (I-4),

[0068] Formula (I-5), and

[0069] Formula (I-6). In some embodiments of the present invention, the first flame retardant (C) has the structure of formula (I-1).

[0070] Compared to other DOPO-based flame retardants, the first flame retardant (C) used in this invention comprises an aryl-substituted ethyl crosslinking group. Without being theoretically limited, it is believed that the shorter chain of this crosslinking group results in better rigidity for the first flame retardant (C); and the aryl substituents on the ethyl acetate create a significant steric barrier effect, thus endowing the first flame retardant (C) with good chemical stability and low volatility. Therefore, electronic materials made from the resin composition of this invention can possess superior flame-retardant properties.

[0071] Studies have found that bismaleimide resin (B) and the first flame retardant (C) can exert a special synergistic effect, enabling the resin composition of the present invention to not only improve the poor adhesion between laminates and metal foils caused by the addition of bismaleimide to epoxy resin systems, but also to provide the laminates with good laminate characteristics and dielectric properties. Furthermore, the weight ratio of bismaleimide resin (B) to the first flame retardant (C) is preferably 1:6 to 6:1, more preferably 1:5 to 5:1, for example 1:6, 1:5, 1:4, 1:3, 1:2, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, or within a range consisting of any two of the above values. When the weight ratio of bismaleimide resin (B) to the first flame retardant (C) is within the range described above, the electronic materials made from the resin composition of the present invention can have better tear strength, electrical properties after moisture absorption, and filler properties.

[0072] Generally, based on the solid content of the resin composition, the content of the first flame retardant (C) can range from 5% to 35% by weight, for example, 5% by weight, 5.5% by weight, 6% by weight, 6.5% by weight, 7% by weight, 7.5% by weight, 8% by weight, 8.5% by weight, 9% by weight, 9.5% by weight, 10% by weight, 10.5% by weight, 11% by weight, 11.5% by weight, 12% by weight, 12.5% ​​by weight, 13% by weight, 13.5% by weight, 14% by weight, 14.5% by weight, 15% by weight, 15.5% by weight, 16% by weight, 16.5% by weight, 17% by weight, 17.5% by weight, 18% by weight, 18.5% by weight, 19% by weight, 19.5% by weight. 20% by weight, 20.5% by weight, 21% by weight, 21.5% by weight, 22% by weight, 22.5% by weight, 23% by weight, 23.5% by weight, 24% by weight, 24.5% by weight, 25% by weight, 25.5% by weight, 26% by weight, 26.5% by weight, 27% by weight, 27.5% by weight, 28% by weight, 28.5% by weight, 29% by weight, 29.5% by weight, 30% by weight, 30.5% by weight, 31% by weight, 31.5% by weight, 32% by weight, 32.5% by weight, 33% by weight, 33.5% by weight, 34% by weight, 34.5% by weight, or 35% by weight, or within the range of any two of the above values, but the present invention is not limited thereto.

[0073] 1.3. Other optional ingredients as needed

[0074] In addition to the above-mentioned components, the resin composition of the present invention may further contain other selected components to specifically improve the physicochemical properties of electronic materials made from the resin composition, or to improve the processability of the resin composition during manufacturing. The selected components of the resin composition of the present invention may be any additives well known in the art, such as curing accelerators, curing agents, fillers, dispersants, elastomers, toughening agents, viscosity modifiers, flame retardants other than the first flame retardant (C), plasticizers, coupling agents, etc. The use of such additives is something that those skilled in the art, upon viewing the disclosure of this specification, can do as needed based on their ordinary knowledge, and is not the focus of the present invention; therefore, it will not be described in detail here. The following description exemplifies curing accelerators, curing agents, and fillers.

[0075] 1.3.1. Hardening agent accelerator

[0076] Curing accelerators promote the reaction of epoxy functional groups and lower the curing temperature of resin compositions. Curing accelerators can be any substance that promotes the ring-opening of epoxy functional groups and lowers the curing temperature; examples include tertiary amines, quaternary amines, imidazole compounds, and pyridine compounds. The aforementioned curing accelerators can be used alone or in combination. In some embodiments of the present invention, the curing accelerator is an imidazole compound, a pyridine compound, or a combination thereof. Examples of imidazole compounds include, but are not limited to, 2-methylimidazole (2MI), 2-ethyl-4-methylimidazole (2E4MZ), and 2-phenylimidazole (2PI). Examples of pyridine compounds include, but are not limited to, 2,3-diaminopyridine, 2,5-diaminopyridine, 2,6-diaminopyridine, 4-dimethylaminopyridine, 2-amino-3-methylpyridine, 2-amino-4-methylpyridine, and 2-amino-3-nitropyridine. In some embodiments of the present invention, 2-phenylimidazole and 2-ethyl-4-methylimidazole are used as curing accelerators.

[0077] Generally, the content of the curing accelerator, based on the solid content of the resin composition, can be from 0.01% to 0.1% by weight, for example 0.01% by weight, 0.02% by weight, 0.03% by weight, 0.04% by weight, 0.05% by weight, 0.06% by weight, 0.07% by weight, 0.08% by weight, 0.09% by weight, or 0.1% by weight, or within the range of any two of the above values, but the present invention is not limited thereto.

[0078] 1.3.2. Hardener

[0079] The curing agent can be any known curing agent suitable for epoxy resins, such as hydroxyl-containing compounds, amine-containing compounds, acid anhydride compounds, and reactive ester compounds. Examples of curing agents include, but are not limited to: cyanate ester resins, benzoxazine resins, phenolic resins (PN), styrene-maleic anhydride resins (SMA), dicyandiamine (Dicy), diaminodiphenyl sulfone (DDS), aminotriazaphenolic resins (ATN), diaminodiphenylmethane, styrene-vinylphenol copolymers, and combinations thereof. In some embodiments of the invention, benzoxazine resins, styrene-maleic anhydride resins, or combinations thereof are used as curing agents.

[0080] Generally, the content of the hardener, based on the solid content of the resin composition, can be from 5% to 30% by weight, for example, 5% by weight, 6% by weight, 7% by weight, 8% by weight, 9% by weight, 10% by weight, 11% by weight, 12% by weight, 13% by weight, 14% by weight, 15% by weight, 16% by weight, 17% by weight, 18% by weight, 19% by weight, 20% by weight, 21% by weight, 22% by weight, 23% by weight, 24% by weight, 25% by weight, 26% by weight, 27% by weight, 28% by weight, 29% by weight, or 30% by weight, or within the range of any two of the above values, but the present invention is not limited thereto.

[0081] 1.3.3. Packing

[0082] Examples of fillers include, but are not limited to, organic or inorganic fillers selected from the following group: silica (such as spherical, fused, non-fused, porous, or hollow silica), alumina, magnesium oxide, magnesium hydroxide, calcium carbonate, talc, clay, aluminum nitride, boron nitride, aluminum hydroxide, silicon aluminum carbide, silicon carbide, sodium carbonate, titanium dioxide, zinc oxide, zirconium oxide, quartz, diamond, diamond-like particles, graphite, calcined kaolin, baiji, mica, hydrotalcite, polytetrafluoroethylene (PTFE) powder, glass beads, ceramic whiskers, carbon nanotubes, nano-scale inorganic powders, and combinations thereof. In some embodiments of the invention, silica fillers are used.

[0083] Generally, the filler content, based on the solid content of the resin composition, can be from 0% to 45% by weight, for example, 1% by weight, 3% by weight, 5% by weight, 7% by weight, 10% by weight, 13% by weight, 15% by weight, 17% by weight, 20% by weight, 23% by weight, 25% by weight, 27% by weight, 30% by weight, 33% by weight, 35% by weight, 37% by weight, 40% by weight, 43% by weight, or 45% by weight, or within the range of any two of the above values, but the present invention is not limited thereto.

[0084] 1.4. Preparation of Resin Composition

[0085] Regarding the preparation of the resin composition of the present invention, the components of the resin composition, including (A) epoxy resin, (B) bismaleimide resin, (C) a first flame retardant, and other optional components as needed, are uniformly mixed and dissolved or dispersed in a solvent using a stirrer to form a varnish-like form for subsequent processing. The solvent can be any inert solvent capable of dissolving or dispersing the components of the resin composition without reacting with them. For example, solvents that can be used to dissolve or disperse the components of the resin composition include, but are not limited to, toluene, γ-butyrolactone, methyl ethyl ketone, cyclohexanone, butanone, acetone, xylene, methyl isobutyl ketone, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), and N-methylpyrrolidone (NMP), and the aforementioned solvents can be used alone or in combination. There are no particular limitations on the amount of solvent used; in principle, it is sufficient to ensure that all components of the resin composition are uniformly dissolved or dispersed therein. In some embodiments of the present invention, a mixture of methyl ethyl ketone and N,N-dimethylformamide is used as the solvent.

[0086] 2. Prepreg

[0087] This invention also provides a prepreg made from the above-described resin composition, wherein the prepreg is obtained by impregnating a substrate with the above-described resin composition or coating a substrate with the above-described resin composition, and then drying the impregnated or coated substrate. Commonly used substrates include, but are not limited to, paper, cloth, or felt made from materials selected from the group consisting of: paper fibers, glass fibers, quartz fibers, organic polymer fibers, carbon fibers, and combinations thereof. Examples of organic polymer fibers include, but are not limited to, high-modulus polypropylene (HMPP) fibers, polyamide fibers, ultra-high molecular weight polyethylene (UHMWPE) fibers, and liquid crystal polymers (LCP), and the cloth made from the group of materials can be woven or non-woven. In some embodiments of this invention, 2116 reinforced glass fiber cloth is used as a reinforcing material and heated and dried at 175°C for 2 to 15 minutes (B-stage) to obtain a prepreg in a semi-cured state.

[0088] 3. Metal foil laminates and printed circuit boards

[0089] The present invention also provides a metal foil laminate, which is prepared by laminating the prepreg described above with a metal foil, or by coating the resin composition described above onto a metal foil and then drying the coated metal foil. In the case of preparing a metal foil laminate using a prepreg, multiple layers of the prepreg described above can be stacked, and then a metal foil (such as a copper foil) is stacked on at least one outer surface of the dielectric layer formed by the stacked prepregs to provide a laminate, and the laminate is subjected to a hot pressing operation to obtain the metal foil laminate.

[0090] The aforementioned metal foil laminate can be further patterned on its outer metal foil to form a printed circuit board.

[0091] 4. Example

[0092] 4.1. Measurement Method Description

[0093] The present invention will now be further illustrated by the following specific embodiments, wherein the measuring instruments and methods used are as follows:

[0094] [Glass Transfer Temperature (Tg) Test]

[0095] The copper foil on both sides of the multilayer board used for evaluation was removed by etching. The resulting unclad board had its glass transition temperature (Tg) measured using a thermomechanical analyzer (TMA). The glass transition temperature test specification was IPC-TM-650.2.4.24C, issued by the Institute for Interconnecting and Packaging Electronic Circuits (IPC).

[0096] [Measurement of Coefficient of Thermal Expansion (z-CTE)]

[0097] The coefficient of thermal expansion (z-CTE) along the Z-axis (thickness direction) of a fully cured thermosetting resin composition was measured using a thermomechanical analyzer (TMA). The test procedure was as follows: A 5 mm × 5 mm × 1.5 mm fully cured thermosetting resin composition was prepared as the test sample. The initial temperature was set to 30°C, the final temperature to 330°C, the heating rate to 10°C / min, and the load to 0.05 N. Under these conditions, thermomechanical analysis was performed on the test sample in expansion / compression mode. The thermal expansion per 1°C within the temperature range of 30°C to 330°C was measured, and the average value was taken. The unit of z-CTE is %.

[0098] [Tear Strength Test]

[0099] Tear strength refers to the adhesion of a metal foil to a prepreg that has been thermo-laminated. It is expressed by the force required to tear a 1 / 8-inch wide (0.5 ounce) copper foil vertically from the surface of the board. The unit of tear strength is pounds-force per inch (lbf / in).

[0100] [Heat Resistance Test]

[0101] According to the IPC-TM-650 2.4.24.1 specification, the metal foil laminate was immersed in a 288°C solder bath, and the time required until the board burst was recorded.

[0102] [Dimensional stability test]

[0103] Four semi-cured sheets were laminated to prepare the sample for testing. According to IPC-TM-650 2.4.24.5, the coefficient of thermal expansion (CTE) α1 and the rate of change of CTE along the Z-axis (total z-CTE) of the sample were measured using a thermal mechanical analyzer (TMA) at temperatures below Tg. α1 was measured in the temperature range of 50°C to 120°C, and the unit is ppm / °C. Total z-CTE was measured in the temperature range of 50°C to 260°C, and the unit is %.

[0104] [Warpage Test]

[0105] According to the IPC TM-650-2.4.22 specification, the metal foil laminate was etched on one side, the warping phenomenon of the laminate was observed, and the warping rate was calculated.

[0106] [Glue Filling Test]

[0107] To test resin flow, 1037 glass fiber cloth impregnated with the resin composition was used to provide a semi-cured sheet. The semi-cured sheets were stacked in the following order: steel plate / copper foil / semi-cured sheet / perforated pattern / copper foil / steel plate. After stacking, the sheets were placed in a press and hot-pressed for 120 minutes at a temperature of 210±5℃, a surface pressure of 39 kg, and a heating rate of 2.5℃ / min. After hot pressing, the perforated pattern was removed and cooled to room temperature. The percentage of filled holes was calculated as: (total number of filled holes / total number of holes) × 100%.

[0108] [Flame Retardancy Test]

[0109] Using the UL94V: Vertical Burning Test Method, a metal foil laminate was fixed vertically and burned with a Bunsen burner to compare its self-extinguishing and combustion-supporting characteristics. The flame retardancy ratings were ranked as follows: V0 > V1 > V2.

[0110] [Measurement of dielectric constant (Dk) and dielectric loss factor (Df)]

[0111] According to IPC-TM-650 2.5.5.13, the dielectric constant (Dk) and dielectric loss factor (Df) were calculated using a split post dielectric resonator (SPDR) at an operating frequency of 10 GHz. The resin content (RC) of the prepreg used for testing was 55%.

[0112] [Measurement of dielectric constant (Dk) and dielectric loss factor (Df) after moisture absorption]

[0113] Using a pressure cooker, after standing for 5 hours at 121°C and 2 atmospheres, the values ​​of dielectric constant (Dk) and dielectric loss factor (Df) after moisture absorption were measured according to the aforementioned method [Measuring dielectric constant (Dk) and dielectric loss factor (Df)].

[0114] 4.2. List of raw materials used in the examples and comparative examples: ,

[0115] 4.3. Preparation of Resin Composition

[0116] According to the components and proportions shown in Tables 1-1, 1-2 and 2, the components were mixed at room temperature using a stirrer, and methyl ethyl ketone and N,N-dimethylformyl (both purchased from Genxiang Industrial Co., Ltd.) were added. The resulting mixture was then stirred at room temperature for 60 to 120 minutes to obtain the resin compositions of Examples E1 to E19 and Comparative Examples CE1 to CE7.

[0117] Table 1-1 ,

[0118] Table 1-2 ,

[0119] Table 2 ,

[0120] 4.4. Preparation and performance testing of metal foil laminates

[0121] Metal foil laminates of Examples E1 to E19 and Comparative Examples CE1 to CE7 were prepared using the obtained resin compositions. First, glass fiber cloth (model: 2116, thickness: 0.08 mm) was impregnated with the resin compositions of Examples E1 to E19 and Comparative Examples CE1 to CE7 using a roller coater, and the thickness of the glass fiber cloth was controlled to a suitable level. Next, the impregnated glass fiber was placed in a dryer at 175°C and dried for 2 to 15 minutes to obtain a prepreg in a semi-cured state (B-stage) (the resin content of the prepreg was 55%). Then, several prepregs were laminated, and a 0.5 oz copper foil was laminated on the outermost layer of each side, followed by high-temperature hot pressing curing in a hot press. The hot-pressing conditions are as follows: heat up to 200°C to 220°C at a heating rate of 3.0°C / min, and at this temperature, hot-press for 180 minutes at a total pressure of 15 kg / cm² (initial pressure of 8 kg / cm²).

[0122] The properties of the metal foil laminates of Examples E1 to E19 and Comparative Examples CE1 to CE7 were measured according to the measurement methods described above, including glass transition temperature (Tg), coefficient of thermal expansion, tear strength, heat resistance, dimensional stability, processability (including warpage and filler properties), flame retardancy, dielectric constant (Dk) and dielectric loss factor (Df), and dielectric constant (Dk) and dielectric loss factor (Df) after moisture absorption. The results are recorded in Tables 3-1, 3-2 and 4.

[0123] Table 3-1 ,

[0124] Table 3-2 ,

[0125] Table 4

[0126] As shown in Tables 3-1, 3-2, and 4, the metal foil laminates made from the resin composition of the present invention exhibit good laminate properties and dielectric properties. In contrast, Comparative Examples CE1 to CE4 and CE7 show that when a flame retardant commonly used in the art is substituted for the first flame retardant (C), the resulting metal foil laminates have poor tear strength, dimensional stability, warpage, and filler properties, and the changes in Dk and Df after moisture absorption are large. Comparative Example CE5 shows that, without the use of any flame retardant, the metal foil laminate has poor tear strength and flame retardancy, and the changes in Dk and Df after moisture absorption are large. Comparative Example 6 shows that when bismaleimide resin (B) is not used, the resulting metal foil laminate has poor Tg, heat resistance, and filler properties.

[0127] The above results clearly demonstrate that the desired synergistic effect can only be achieved by combining the first flame retardant (C) and bismaleimide resin (B) in the epoxy resin composition. This improves the poor adhesion between the laminate and the metal foil caused by the addition of bismaleimide to the epoxy resin system and provides the laminate with good laminate properties and dielectric properties.

[0128] The above embodiments are merely illustrative of the principles and effects of the present invention and to illustrate its technical features, and are not intended to limit the scope of protection of the present invention. Any changes or arrangements that can be easily made by those skilled in the art without departing from the technical principles and spirit of the present invention are within the scope claimed by the present invention.

Claims

1. A resin composition, characterized in that, It includes: (A) Epoxy resin; (B) Bismaleimide resin; and (C) The first flame retardant, having the structure of formula (I): Equation (I), in, Ar is C3 to C 18 heteroaryl or C6 to C 18 Aryl; R1 is hydrogen or C1 to C2. 18 Alkyl groups; and R2 and R3 are each independently hydrogen, C1 to C3. 18 Alkyl, C3 to C 18 heteroaryl, or C6 to C 18 Aryl; in, The weight ratio of the bismaleimide resin (B) to the first flame retardant (C) is 5:1 to 1:

5.

2. The resin composition according to claim 1, characterized in that, The epoxy resin (A) is selected from the following group: bisphenol type epoxy resins, phenolic type epoxy resins, stilbene type epoxy resins, epoxy resins containing a triazine backbone, epoxy resins containing a pyridine backbone, pyromethane type epoxy resins, cycloaliphatic type epoxy resins, biphenyl type epoxy resins, biphenyl aralkyl type epoxy resins, naphthalene type epoxy resins, dicyclopentadiene type epoxy resins, alicyclic epoxy resins, and combinations thereof.

3. The resin composition as described in claim 1, characterized in that, The bismaleimide resin (B) has the structure shown by formula (II): Equation (II), R4 is selected from the following groups: -CH2- , , , , , ,and , Represents the connection site.

4. The resin composition according to claim 1, characterized in that, The bismaleimide resin (B) is selected from the following group: 1,2-bismaleimide ethane, 1,6-bismaleimide hexane, 1,3-bismaleimide benzene, 1,4-bismaleimide benzene, 2,4-bismaleimide toluene, 4,4'-bismaleimide diphenylmethane, 4,4'-bismaleimide diphenyl ether, 3,3'-bismaleimide diphenyl sulfone, 4,4'-bismaleimide diphenyl 4,4'-bismaleimide dicyclohexylmethane, 3,5-bis(4-maleimide phenyl)pyridine, 2,6-bismaleimide pyridine, 1,3-bis(maleimide methyl)cyclohexane, 1,3-bis(maleimide methyl)benzene, 1,1-bis(4-maleimide phenyl)cyclohexane, 1,3-bis(dichloromaleimide)benzene, 4,4'-bisciconimide diphenylmethane, 2,2-bis... (4-maleimide-phenyl)propane, 1-phenyl-1,1-bis(4-maleimide-phenyl)ethane, α,α-bis(4-maleimide-phenyl)toluene, 3,5-bismaleimide-1,2,4-triazole, N,N'-epenylethylbismaleimide, N,N'-hexamethylenebismaleimide, N,N'-m-epenylphenylbismaleimide, N,N'-p-epenylphenylbismaleimide, N,N'-4, 4'-Diphenylmethane bismaleimide, N,N'-4,4'-diphenyl ether bismaleimide, N,N'-4,4'-diphenyl sulfone bismaleimide, N,N'-4,4'-dicyclohexylmethane bismaleimide, N,N'-α,α'-4,4'-dimethylenecyclohexane bismaleimide, N,N'-m-xylene bismaleimide, N,N'-4,4'-diphenylcyclohexane bismaleimide, and combinations thereof.

5. The resin composition according to claim 1, characterized in that, The first flame retardant (C) is selected from the following group: Equation (I-1), Equation (I-2), Equation (I-3), Equation (I-4), Equation (I-5), Formula (I-6) and its combinations.

6. The resin composition according to claim 1, characterized in that, Based on the solid content of the resin composition, the content of the bismaleimide resin (B) and the first flame retardant (C) is independently 5% to 35% by weight.

7. The resin composition according to claim 1, characterized in that, The content of epoxy resin (A) is 3% to 15% by weight, based on the solid content of the resin composition.

8. The resin composition according to claim 1, characterized in that, It further includes curing agents selected from the following group: cyanate ester resins, benzoxazine resins, phenolic resins, styrene-maleic anhydride resins, dicyandiamine, diaminodiphenyl sulfone, aminotriazine phenolic resins, diaminodiphenylmethane, styrene-vinylphenol copolymers, and combinations thereof.

9. The resin composition according to claim 1, characterized in that, It also includes hardening accelerators selected from the following groups: imidazole compounds, pyridine compounds, and combinations thereof.

10. The resin composition according to claim 1, characterized in that, It also includes fillers selected from the following groups: silica, alumina, magnesium oxide, magnesium hydroxide, calcium carbonate, talc, clay, aluminum nitride, boron nitride, aluminum hydroxide, silicon aluminum carbide, silicon carbide, sodium carbonate, titanium dioxide, zinc oxide, zirconium oxide, quartz, diamond, diamond-like material, graphite, calcined kaolin, baiji, mica, hydrotalcite, polytetrafluoroethylene powder, glass beads, ceramic whiskers, carbon nanotubes, nano-scale inorganic powders, and combinations thereof.

11. A semi-cured sheet, characterized in that, It is prepared by impregnating or coating a substrate with a resin composition as described in any one of claims 1 to 10, and drying the impregnated or coated substrate.

12. A metal foil laminate, characterized in that, It is prepared by laminating the prepreg as described in claim 11 with a metal foil, or by coating the metal foil with the resin composition as described in any one of claims 1 to 10 and drying the coated metal foil.

13. A printed circuit board, characterized in that, It is made from the metal foil laminate as described in claim 12.

Citation Information

Patent Citations

  • DOPO derivative flame retardants

    WO2010135398A1

  • DOPO derivatives as well as preparation method and application thereof

    CN104086593A

  • Resin composition, and pre-preg, metal-clad laminate and printed circuit board prepared using the same

    CN109467888A