Segmented composite capillary superthin heat pipe and method of manufacturing the same

By using a segmented composite capillary core composed of copper inverse opal and copper fiber bundles in an ultrathin heat pipe, the problem of single wicking structures being unable to balance capillary force and permeability is solved, thus achieving high-efficiency heat transfer performance of the heat pipe.

CN117628955BActive Publication Date: 2026-11-24WUHAN UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311788690.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2026-11-24
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

In the heat transfer process, the single wick structure of existing ultrathin heat pipes makes it difficult to balance capillary force and permeability, resulting in low heat transfer efficiency. Furthermore, the internal space is limited after the flattening process, which affects the performance of the heat pipe.

Method used

A segmented composite capillary core is formed by combining copper inverse opal and copper fiber bundles. Copper inverse opal is used in the evaporation and condensation sections, while copper fiber bundles are used in the insulation section, thus forming a segmented composite capillary core that enhances capillary force and permeability and optimizes heat transfer performance.

Benefits of technology

It improves the heat transfer performance of the heat pipe, enhances the flow and return speeds of steam and liquid, reduces heat transfer resistance, and ensures uniform heat distribution and efficient heat transfer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117628955B_ABST
    Figure CN117628955B_ABST
Patent Text Reader

Abstract

This invention discloses a segmented composite capillary ultrathin heat pipe and its manufacturing method. The heat pipe includes a shell, a copper mesh inside the shell, a segmented composite capillary, and a working fluid filled inside the shell. The segmented composite capillary includes copper inverse opal and copper fiber bundles. The copper mesh is attached and fixed to the longitudinal sidewalls of the shell. The copper inverse opal is located at both ends of the shell, stacked in a face-centered cubic pattern and filled with uniform spherical pores. Circular pores are formed at the junctions of adjacent spherical pores. The copper fiber bundles are composed of multiple copper fibers stacked together. The longitudinal ends of the copper fiber bundles are connected to the copper inverse opal, and the sides in the thickness direction are connected to the copper mesh. At least two copper fiber bundles are distributed along the width of the shell. Vapor channels are formed between adjacent copper fiber bundles and between the copper fiber bundles and the sidewalls of the shell. This invention ensures that the capillary force and permeability of the heat pipe capillary simultaneously meet the requirements, thus optimizing and improving heat transfer performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to ultrathin heat pipes, specifically to a segmented composite capillary ultrathin heat pipe and its manufacturing method. Background Technology

[0002] Electronic devices are rapidly developing towards high performance and miniaturization. If the heat generated during their operation cannot be dissipated in time, their failure rate will increase significantly. Ultra-thin heat pipes, with their simple and reliable design, extremely high thermal conductivity and good isothermal properties, have become the ideal choice for heat dissipation of high heat flux electronic devices. In order to adapt to the narrow heat dissipation space inside thin and light electronic products, ultra-thin heat pipes usually adopt a flat shape with a thickness of less than 2mm.

[0003] The internal structure of an ultrathin heat pipe generally includes an evaporation section, a condensation section, and an adiabatic section. Its heat dissipation principle is as follows: In the evaporation section, the working liquid inside the tube is heated and evaporates, carrying away heat. The vapor flows from the adiabatic section channel to the condensation section, condenses into liquid, and releases latent heat. At the same time, the liquid flows back to the evaporation section under the capillary force of the wick, forming a closed heat transfer cycle, which effectively removes a large amount of heat from the heat source.

[0004] The heat transfer performance of ultrathin heat pipes is mainly affected by the wick. Traditional wicks include three main categories: sintered powder wicks, grooved wicks, and mesh wicks. The design goal of these wicks is to provide strong capillary force, good permeability, and increased heat exchange area. However, a problem exists with a single wick structure: the smaller the equivalent pore size, the greater the capillary force, but this also leads to increased backflow resistance and decreased permeability, making it difficult to achieve both high capillary force and high permeability, thus limiting the improvement of heat pipe performance.

[0005] To overcome the problems of a single wick structure, many ultrathin heat pipes with composite capillary wicks have been designed. However, in the current process of flattening heat pipes, the volume of the cavity inside the tube is significantly reduced, causing the composite capillary wick to occupy most of the space inside the tube. This limits the total amount of working liquid that can be filled in. Furthermore, the narrow flow path of the gaseous working fluid during heat transfer affects the smooth transfer of latent heat. At the same time, when the liquid comes into contact with the vapor, heat is transferred to the liquid, increasing the heat transfer resistance of the adiabatic section and reducing the heat transfer efficiency. This may lead to uneven local temperature distribution, which in turn affects the overall performance of the heat pipe.

[0006] The working principle of ultra-thin heat pipes reveals that the evaporation and condensation sections require sufficient capillary force and contact area, while the adiabatic section needs a spacious gas-liquid separation channel. Capillary force rapidly draws liquid from the condensation section back to the evaporation section, and the reflux rate and reflux velocity are the decisive factors determining the evaporation efficiency of the evaporation section. Current ultra-thin heat pipes often employ methods that increase the thickness of the capillary structure; however, this increases the reflux rate while simultaneously compressing the space of the vapor channel, reducing the heat transfer limit. Summary of the Invention

[0007] The purpose of this invention is to provide a segmented composite capillary ultrathin heat pipe and its manufacturing method. The segmented composite capillary is composed of copper inverse opal and copper fiber bundles, which ensures that the capillary force and permeability of the heat pipe capillary meet the requirements at the same time, thereby optimizing and improving the heat transfer performance.

[0008] The technical solution adopted in this invention is: A segmented composite capillary ultrathin heat pipe includes a shell, a copper mesh inside the shell, a segmented composite capillary, and a working fluid filled inside the shell. The segmented composite capillary includes copper inverse opal and copper fiber bundles. The shell is flat, internally sealed, and made of copper alloy. The copper mesh is attached and fixed to the longitudinal sidewalls of the shell. The copper inverse opal is located at both ends of the shell, with one side attached and fixed to the inner wall of the shell end face and the other side connected to the copper mesh. The copper inverse opal is stacked in a face-centered cubic form and has uniform spherical pores inside, with circular pores formed at the junction of adjacent spherical pores. The copper fiber bundle is composed of multiple copper fibers stacked together. The longitudinal ends of the copper fiber bundle are connected to the copper inverse opal, and the sides in the thickness direction are connected to the copper mesh. At least two copper fiber bundles are distributed along the width direction of the shell, and the gaps between adjacent copper fiber bundles and between the copper fiber bundles and the sidewalls of the shell form vapor channels.

[0009] Preferably, the cross-section of the tube shell is rectangular.

[0010] Preferably, the thickness of the tube shell is 0.4mm-2mm, the wall thickness of the tube shell is 0.05mm-0.1mm, the thickness of the copper mesh is 0.01mm-0.1mm, the number of copper inverse opal structure layers exceeds 20, the diameter of the spherical holes is 0.005mm-0.02mm, and the diameter of the copper fibers ranges from 0.02mm to 0.08mm.

[0011] Preferably, the steam channel between adjacent copper fiber bundles is designated as the inner steam channel, and the steam channel between the copper fiber bundle and the sidewall of the tube shell is designated as the outer steam channel. The width of the outer steam channel is greater than or equal to the width of the inner steam channel.

[0012] Preferably, the copper fibers in the same row are closely arranged, and the copper fibers in adjacent rows are aligned and closely arranged; or, the copper fibers in the same row are closely arranged, and the copper fibers in adjacent rows are staggered and closely arranged.

[0013] Preferably, the working fluid is deionized water.

[0014] The manufacturing method of the above-mentioned segmented composite capillary ultrathin heat pipe is as follows: S1. Assemble the copper mesh and copper inverse opal at one end: Take a tube shell with open ends, insert the annular copper mesh into the tube shell using a mandrel, and after removing the mandrel, the copper mesh expands outward due to elasticity and adheres tightly to the side walls of the tube shell. Weld the copper mesh to the tube shell. After the tube shell is hydrophilic, immerse one end in a polystyrene ball solution with a diameter of 0.005mm-0.02mm. Use the vertical deposition method to self-assemble a layered ordered structure on the inner wall of the tube. After sintering at 100-105℃, fill the tube with copper alloy material by electrodeposition. Immerse this end in tetrahydrofuran solvent to dissolve the polystyrene balls and obtain an ordered copper inverse opal. S2. Assemble the copper fiber bundle and the copper inverse opal at the other end: Insert the prepared copper fiber bundle into the tube shell and make contact with the copper inverse opal at the front end. The two sides of the copper fiber bundle are tightly attached to the copper mesh with organic adhesive. The copper inverse opal is made on the inner wall of the tube at the other end by means of step S1, while the outer wall of the tube is polished smooth. S3. By high-temperature sintering or electric welding, the copper fiber bundle and the copper inverse opal at both ends are tightly bonded to obtain a segmented composite capillary core, and the tube shell is sintered into an integral structure at high temperature. S4. Tube shell treatment and filling: Reduce the size of both ends of the tube shell and seal one end, leaving an opening at the other end for filling and vacuuming. After annealing the tube shell, fill the tube shell with working fluid, then vacuum the tube shell, and finally seal the opening. S5. Molding heat pipe: Bend and flatten the tube shell to the set thickness as needed.

[0015] Preferably, the method for preparing copper inverse opal is as follows: First, prepare a solution of polystyrene spheres and ethanol, vertically immerse one end of a hydrophilically treated tube shell model into the solution, and evaporate and deposit the polystyrene spheres at a temperature of 50-60°C to form an ordered array; or prepare a solution of polystyrene spheres and water, vertically immerse one end of a hydrophilically treated tube shell model into the solution, heat it at a temperature of 50-60°C for a period of time, and then lift it out, leaving a liquid film on the tube wall. After evaporation, an ordered array of polystyrene spheres is formed. Then, after sintering at 100-105°C, the contact points between adjacent polystyrene spheres are expanded to become contact surfaces. Then, copper alloy material is filled into the gaps between the models by electrodeposition. Finally, the prepared model is immersed in tetrahydrofuran solvent to dissolve the polystyrene spheres, thereby obtaining an ordered copper inverse opal.

[0016] Preferably, the welding method for copper inverse opal and copper mesh is as follows: the copper inverse opal and copper mesh are welded together by resistance welding in a vacuum environment at 850°C, wherein the vacuum environment is a mixed gas environment containing 95% nitrogen and 5% hydrogen.

[0017] Preferably, when flattening the tube shell, the tube shell is maintained at 105-110°C to prevent wrinkles from forming during flattening.

[0018] The beneficial effects of this invention are as follows: In this invention, the copper mesh increases the steam flow rate, the copper inverse opal can fill more working fluid without affecting capillary force, has a larger surface area, and improves the heat transfer interface. The copper fiber bundles increase the liquid return flow rate and velocity, and can also support the tube shell. The large and dispersed steam channels can ensure that the steam and liquid do not come into contact with each other. The segmented composite capillary core composed of copper inverse opal and copper fiber bundles ensures that the capillary force and permeability of the heat pipe capillary core meet the requirements at the same time, thus optimizing and improving the heat transfer performance. Attached Figure Description

[0019] Figure 1 This is a schematic longitudinal section of the segmented composite capillary ultrathin heat pipe in Embodiment 1 of the present invention.

[0020] Figure 2 This is a cross-sectional schematic diagram of the segmented composite capillary ultrathin heat pipe in Embodiment 1 of the present invention.

[0021] Figure 3 This is a three-dimensional structural diagram of the copper inverse opal in Embodiment 1 of the present invention. For ease of observation, only three layers are shown.

[0022] Figure 4 This is a three-dimensional structural diagram of the copper fiber bundle in Embodiment 1 of the present invention.

[0023] Figure 5 This is a cross-sectional schematic diagram of the copper fiber bundle in Embodiment 1 of the present invention.

[0024] Figure 6 This is a schematic cross-sectional view of the copper fiber bundle in Embodiment 2 of the present invention.

[0025] In the figure: 1-shell; 11-sidewall; 12-end face; 2-copper mesh; 3-copper inverse opal; 31-spherical hole; 32-circular pore; 4-copper fiber bundle; 41-copper fiber; 5-steam channel; 51-inner steam channel; 52-outer steam channel. Detailed Implementation

[0026] The present invention will be further described below with reference to the accompanying drawings and embodiments.

[0027] Example 1 This embodiment discloses a segmented composite capillary ultrathin heat pipe, such as Figures 1 to 5As shown: The system includes a shell 1, a copper mesh 2 located inside the shell 1, a segmented composite capillary core, and a working fluid filled inside the shell 1. The segmented composite capillary core includes copper inverse opal 3 and copper fiber bundles 4. The shell 1 is flat, internally sealed, and made of copper alloy. The copper mesh 2 is attached and fixed to the longitudinal sidewalls 11 of the shell 1. The copper inverse opal 3 is located at both ends of the shell 1, with one side attached and fixed to the inner wall of the end face 12 of the shell 1, and the other side connected to the copper mesh 2 around its perimeter. The copper inverse opal 3 is stacked in a face-centered cubic form and is filled with uniform spherical holes 31. Circular pores 32 are formed at the junction of adjacent spherical holes 31. The copper fiber bundle 4 is formed by stacking multiple copper fibers 41. The two ends of the copper fiber bundle 41 are connected to the copper inverse opal 3 respectively, and the two sides in the thickness direction are connected to the copper mesh 2 respectively. At least two copper fiber bundles 4 are distributed along the width direction of the tube shell 1. The gaps between adjacent copper fiber bundles 4 and between the copper fiber bundles 4 and the side wall of the tube shell 1 form a steam channel 5. During operation, the copper inverse opal 3 near the heat source is the evaporation section, the copper inverse opal 3 away from the heat source is the condensation section, and the copper fiber bundle 4 is the insulation section. The working fluid in the pores (spherical pores 31 and circular pores 32) of the copper inverse opal 3 in the evaporation section is heated and evaporated into steam. The steam directly and quickly reaches the copper inverse opal 3 in the condensation section from the steam channel 5 and condenses into liquid, releasing a large amount of heat at the same time. The liquid quickly flows back to the copper inverse opal 3 in the evaporation section from the gaps in the copper fiber bundle 4, and so on.

[0028] In this embodiment, the preferred dimensions of each main component are as follows: the thickness of the shell 1 is 0.4mm-2mm, and the wall thickness of the shell 1 is 0.05mm-0.1mm; the thickness of the copper mesh 2 is 0.01mm-0.1mm; the copper inverse opal 3 has more than 20 structural layers, and the diameter of the spherical hole 31 is 0.005mm-0.02mm; the diameter of the copper fiber 41 is in the range of 0.02mm-0.08mm.

[0029] In this embodiment, the working fluid is preferably deionized water, which is a liquid with good material compatibility with the metal tube, high latent heat of vaporization, and high specific heat capacity.

[0030] like Figure 1 and Figure 2 As shown, in this embodiment, the steam channel 5 between adjacent copper fiber bundles 4 is defined as the inner steam channel 51, and the steam channel 5 between the copper fiber bundle 4 and the side wall 11 of the tube shell 1 is defined as the outer steam channel 52. Preferably, the width of the outer steam channel 52 is greater than or equal to the width of the inner steam channel 51.

[0031] like Figure 2 As shown, in this embodiment, the cross-section of the shell 1 is rectangular.

[0032] like Figure 4 and Figure 5As shown, in this embodiment, the copper fibers 41 in the same row are closely arranged, and the copper fibers 41 in adjacent rows are aligned and closely arranged. Example 2 This embodiment provides another arrangement of the copper fiber bundle 4: as follows: Figure 6 As shown, copper fibers 41 in the same row are closely arranged, while copper fibers 41 in adjacent rows are staggered and closely arranged.

[0033] Example 3 This embodiment provides a method for manufacturing a segmented composite capillary ultrathin heat pipe, including the following steps: S1. Assemble the copper mesh 2 and the copper inverse opal 3 at one end: Take a tube shell 1 with open ends, insert the annular copper mesh into the tube shell 1 using a mandrel, and after the mandrel is pulled out, the copper mesh 2 expands outward due to elasticity and adheres tightly to the side walls of the tube shell 1. Weld the copper mesh 2 to the tube shell 1. After the tube shell 1 is hydrophilic, immerse one end in a polystyrene ball solution with a diameter of 0.005mm-0.02mm. Use the vertical deposition method to self-assemble a layered ordered structure on the inner wall of the tube. After sintering at 100-105℃, fill the tube with copper alloy material by electrodeposition. Immerse this end in tetrahydrofuran solvent to dissolve the polystyrene balls and obtain the ordered copper inverse opal 3. The method for preparing copper inverse opal 3 is as follows: First, prepare a solution of polystyrene spheres and ethanol, vertically immerse one end of the hydrophilically treated tube shell 1 model into it, and evaporate and deposit it at a temperature of 50-60℃ to form an ordered array of polystyrene spheres; or prepare a solution of polystyrene spheres and water, vertically immerse one end of the hydrophilically treated tube shell 1 model into it, heat it at a temperature of 50-60℃ for a period of time and then lift it out, leaving a liquid film on the tube wall, which evaporates to form an ordered array of polystyrene spheres; then, after sintering at 100-105℃, expand the contact points between adjacent polystyrene colloidal spheres to become contact surfaces, and then fill the gaps between the models with copper alloy material by electrodeposition. Finally, immerse the prepared model in tetrahydrofuran solvent to dissolve the polystyrene spheres to obtain ordered copper inverse opal 3.

[0034] The welding method of copper inverse opal 3 and copper mesh 2 is as follows: copper inverse opal 3 and copper mesh 2 are welded together by resistance welding in a vacuum environment at 850℃. The vacuum environment is a mixed gas environment containing 95% nitrogen and 5% hydrogen. S2. Assemble the copper fiber bundle 4 and the copper reverse opal 3 at the other end: Insert the prepared copper fiber bundle 4 into the tube shell 1 and contact the copper reverse opal 3 at the front end. The copper fiber bundle 4 is tightly attached to the copper mesh 2 on both sides by organic adhesive. The copper reverse opal 3 is made on the inner wall of the tube at the other end by the method of step S1, and the outer wall of the tube is polished smooth. S3. By high-temperature sintering or electric welding, the copper fiber bundle 4 and the copper inverse opal 3 at both ends are tightly bonded to obtain a segmented composite capillary core, and the tube shell 1 is sintered into an integral structure at high temperature. S4. Treatment and filling of tube shell 1: Reduce the size of both ends of tube shell 1 and seal one end, leaving an opening at the other end for filling and vacuuming. After annealing tube shell 1 (annealing in a vacuum environment at 600℃ for two hours), fill tube shell 1 with working fluid (filling ratio of 80%-140%), then vacuum tube shell 1, and finally seal the opening. S5. Molding heat pipe: Bend and flatten the tube shell 1 to the set thickness as needed; During the flattening of the tube shell 1, the tube shell 1 is maintained at 105-110℃ to prevent wrinkles from forming during the flattening process.

[0035] In this invention, the copper mesh 2 is used to reduce the flow boundary layer thickness of the reflux steam, increase the steam flow velocity, and provide appropriate support and guiding functions. The copper inverse opal 3 has a highly ordered biomimetic cellular structure with a porosity between 78% and 92%. This design not only allows for the filling of more working fluid without affecting capillary force, providing better anti-clogging performance and maintaining high heat transfer efficiency for a longer period, but also, through the uniform distribution of spherical pores and the three-dimensional interconnected channel structure, has a large surface area, improving the heat transfer interface and further enhancing heat transfer performance. The gaps in the copper fiber bundles 4 have a linear guiding effect on reflux, prompting the condensed working fluid to quickly return to the evaporation end, achieving rapid circulation, increasing the liquid reflux rate and velocity, thereby improving the heat transfer limit of the heat pipe. Furthermore, the copper fiber bundles 4 can support the tube shell, reducing the tube wall thickness requirement. When the heat pipe is subjected to external forces such as collisions, it can effectively prevent tube wall indentation. Moreover, since the copper fiber bundles 4 are distributed along the width direction of the tube shell, they can... By linearly expanding the number of capillary wicks without changing the heat pipe thickness, the heat transfer effect of the heat pipe is further enhanced, making it very convenient to improve according to specific heat transfer requirements. In this invention, a large and dispersed vapor channel 5 is provided inside the heat pipe to ensure that the vapor and liquid do not come into contact with each other. The vapor channel 5 is surrounded by copper fiber bundles 4 and copper mesh 2. The design of copper mesh 2 reduces the boundary layer thickness of vapor flow and increases the vapor flow velocity. Both condensed liquid and evaporated vapor can be quickly transferred to the other end, greatly improving the heat transfer efficiency of the heat pipe. This invention uses a segmented composite capillary wick composed of copper inverse opal 3 and copper fiber bundles 4. Copper inverse opal 3 is used as the core structure in the evaporation and condensation sections, and copper fiber bundles 4 is used as the core structure in the insulation section. This ensures that the capillary force and permeability of the heat pipe capillary wick meet the requirements at the same time, optimizing the heat transfer performance. Furthermore, different models of segmented composite capillary wicks can be formed by combining different specifications of copper inverse opal 3 and copper fiber bundles 4, thereby adjusting the heat transfer performance of the heat pipe.

[0036] The embodiments described above are some, but not all, of the embodiments of this application. The detailed description of the embodiments of this application is not intended to limit the scope of the claimed application, but merely to illustrate selected embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.

Claims

1. A segmented composite capillary wick ultrathin heat pipe, characterized in that: The system includes a shell, a copper mesh inside the shell, a segmented composite capillary core, and a working fluid filled inside the shell. The segmented composite capillary core includes copper inverse opal and copper fiber bundles. The shell is flat, internally sealed, and made of copper alloy. The copper mesh is attached and fixed to the longitudinal sidewalls of the shell. The copper inverse opal is located at both ends of the shell, with one side attached and fixed to the inner wall of the end face of the shell, and the other side connected to the copper mesh. The copper inverse opal is stacked in a face-centered cubic form and has uniform spherical pores inside, with circular pores formed at the junction of adjacent spherical pores. The copper fiber bundle is composed of multiple copper fibers stacked together. The longitudinal ends of the copper fiber bundle are connected to the copper inverse opal, and the sides in the thickness direction are connected to the copper mesh. At least two copper fiber bundles are distributed along the width of the shell, and the gaps between adjacent copper fiber bundles and between the copper fiber bundles and the sidewalls of the shell form steam channels.

2. The segmented composite capillary ultrathin heat pipe as described in claim 1, characterized in that: The cross-section of the tube shell is rectangular.

3. The segmented composite capillary ultrathin heat pipe as described in claim 1, characterized in that: The thickness of the tube shell is 0.4mm-2mm, and the wall thickness of the tube shell is 0.05mm-0.1mm; the thickness of the copper mesh is 0.01mm-0.1mm; the copper inverse opal structure has more than 20 layers, and the diameter of the spherical holes is 0.005mm-0.02mm; the diameter of the copper fibers ranges from 0.02mm-0.08mm.

4. The segmented composite capillary ultrathin heat pipe as described in claim 1, characterized in that: Let the steam channel between adjacent copper fiber bundles be the inner steam channel, and the steam channel between the copper fiber bundle and the side wall of the tube shell be the outer steam channel. The width of the outer steam channel is greater than or equal to the width of the inner steam channel.

5. The segmented composite capillary ultrathin heat pipe as described in claim 1, characterized in that: The copper fibers in the same row are closely arranged, and the copper fibers in adjacent rows are aligned and closely arranged; or, the copper fibers in the same row are closely arranged, and the copper fibers in adjacent rows are staggered and closely arranged.

6. The segmented composite capillary ultrathin heat pipe as described in claim 1, characterized in that: The working fluid is deionized water.

7. The method for manufacturing a segmented composite capillary ultrathin heat pipe as described in any one of claims 1 to 6, characterized in that: S1. Assemble the copper mesh and copper inverse opal at one end: Take a tube shell with open ends, insert the annular copper mesh into the tube shell using a mandrel, and after removing the mandrel, the copper mesh expands outward due to elasticity and adheres tightly to the side walls of the tube shell. Weld the copper mesh to the tube shell. After the tube shell is hydrophilic, immerse one end in a polystyrene ball solution with a diameter of 0.005mm-0.02mm. Use the vertical deposition method to self-assemble a layered ordered structure on the inner wall of the tube. After sintering at 100-105℃, fill the tube with copper alloy material by electrodeposition. Immerse this end in tetrahydrofuran solvent to dissolve the polystyrene balls and obtain an ordered copper inverse opal. S2. Assemble the copper fiber bundle and the copper inverse opal at the other end: Insert the prepared copper fiber bundle into the tube shell and make contact with the copper inverse opal at the front end. The two sides of the copper fiber bundle are tightly attached to the copper mesh with organic adhesive. The copper inverse opal is made on the inner wall of the tube at the other end by means of step S1, while the outer wall of the tube is polished smooth. S3. By high-temperature sintering or electric welding, the copper fiber bundle and the copper inverse opal at both ends are tightly bonded to obtain a segmented composite capillary core, and the tube shell is sintered into an integral structure at high temperature. S4. Tube shell treatment and filling: Reduce the size of both ends of the tube shell and seal one end, leaving an opening at the other end for filling and vacuuming. After annealing the tube shell, fill the tube shell with working fluid, then vacuum the tube shell, and finally seal the opening. S5. Molding heat pipe: Bend and flatten the tube shell to the set thickness as needed.

8. The method for manufacturing a segmented composite capillary ultrathin heat pipe as described in claim 7, characterized in that, The method for preparing copper inverse opal is as follows: First, prepare a solution of polystyrene spheres and ethanol, vertically immerse one end of a hydrophilically treated tube-shell model into the solution, and evaporate and deposit the polystyrene spheres at a temperature of 50-60℃ to form an ordered array of polystyrene spheres; or prepare a solution of polystyrene spheres and water, vertically immerse one end of a hydrophilically treated tube-shell model into the solution, heat it at a temperature of 50-60℃ for a period of time, and then lift it out, leaving a liquid film on the tube wall. After evaporation, an ordered array of polystyrene spheres is formed. Then, after sintering at 100-105℃, the contact points between adjacent polystyrene spheres are expanded to become contact surfaces. Then, copper alloy material is filled into the gaps between the models by electrodeposition. Finally, the prepared model is immersed in tetrahydrofuran solvent to dissolve the polystyrene spheres, resulting in an ordered copper inverse opal.

9. The method for manufacturing a segmented composite capillary ultrathin heat pipe as described in claim 7, characterized in that, The welding method for copper inverse opal and copper mesh is as follows: copper inverse opal and copper mesh are welded together by resistance welding in a vacuum environment at 850℃. The vacuum environment is a mixed gas environment containing 95% nitrogen and 5% hydrogen.

10. The method for manufacturing a segmented composite capillary ultrathin heat pipe as described in claim 7, characterized in that: When flattening the tube shell, maintain the tube shell at 105-110℃ to prevent wrinkles from forming during the flattening process.

Citation Information

Patent Citations

  • Manufacturing method of flexible soft copper / aluminum strip heat tube with multiple fibers distributed in ordered arrays

    CN106979712A

  • Gradient ordered pore porous capillary core ultrathin heat pipe and manufacturing method thereof

    CN111912275A