A molten salt battery, metal / metal chloride electrode and method of making same
The preparation of metal/metal chloride electrodes in molten salt electrolytes via electrochemical chlorination solves the problems of inhomogeneity and complexity in gas-phase chlorination reactions, and achieves efficient, low-cost, and stable battery preparation.
Patent Information
- Application Number
- CN202311616575.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-29
AI Technical Summary
Existing gas-phase chlorination reaction methods for preparing metal/metal chloride electrodes for high-capacity molten salt batteries suffer from problems such as uneven reaction, poor controllability, complex processes, and high costs, which affect the consistency and stability of the batteries.
An electrochemical chlorination method is adopted, which involves electrolysis in a molten salt electrolyte with an active metal as the cathode and a foamed metal as the anode to generate a uniform metal chloride film, simplifying the preparation process and avoiding complex pretreatment and posttreatment.
This method achieves uniformity and consistency in metal/metal chloride electrodes, reduces production costs, improves battery cycle stability and electrode controllability, and simplifies the fabrication process.
Smart Images

Figure CN117637978B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of molten salt electrochemical energy storage technology, specifically relating to a molten salt battery, a metal / metal chloride electrode, and a method for preparing the same. Background Technology
[0002] The rapid development of the new energy industry has placed higher demands on large-scale energy storage technologies. Currently, the demand for large-scale electrochemical energy storage technologies mainly focuses on high safety, long cycle life, and low-cost battery systems. Developing new battery energy storage technologies to meet the needs of the large-scale energy storage market is of great significance. Among the various secondary batteries currently being researched for application in the large-scale energy storage market, molten salt batteries are a highly anticipated technology. This is because molten salt electrolytes have significant cost advantages and are environmentally friendly and pollution-free; they will not burn or explode when exposed to air, thus giving molten salt batteries excellent safety performance. Furthermore, the low-cost electrode materials also make molten salt battery technology highly promising for development and application.
[0003] In molten salt batteries, there is a new type of metal-graphite molten salt battery system. This type of battery uses a metal / metal chloride (N / NCl) structure similar to that in metal-chloride molten salt batteries. x The redox couple serves as the negative electrode of the battery, using an intercalation / deintercalation type graphite electrode Cn[AlCl4] / C n As the positive electrode of a battery, it avoids the problems of metal dendrites and corrosion that exist when a single active metal electrode is used as the negative electrode. It also significantly reduces the cost of electrode materials and better meets the needs of large-scale energy storage. However, the stable preparation of the metal / metal chloride negative electrode in this battery system has been a persistent challenge for the large-capacity production of single-cell batteries. Current research on battery performance and reaction mechanisms mainly employs gas-phase chlorination reactions. By using argon gas containing hydrogen chloride as a carrier gas, a chlorination reaction of metal to metal chloride occurs. By controlling the electrolysis charge, metal / metal chloride negative electrodes with different metal chloride contents can be obtained.
[0004] This gas-phase chlorination method is suitable for research on small-capacity (<1mAh) experimental batteries, but it has significant drawbacks for the production of large-capacity (>100mAh) application batteries. (i) The gas-phase chlorination reaction mainly occurs on the surface of the metal electrode, and the surface condition of the metal electrode (cleanliness, oxide film, corrosion, etc.) affects the uniformity of the chlorination reaction and the reaction products, ultimately leading to unstable output performance of the entire battery. (ii) The controllability of the gas-phase reaction is low, resulting in large differences in the capacity of the formed negative electrode, affecting the consistency of the entire battery. (iii) The process is complex. Due to the high requirements for the surface and the fact that the products formed after the chlorination reaction contain a certain amount of adsorbed water and bound water, the electrode preparation process requires a complex cleaning process and a subsequent inert gas heating and dehydration process. Summary of the Invention
[0005] This invention provides a molten salt battery, a metal / metal chloride electrode, and a method for preparing the same. It simplifies the preparation process of the metal / metal chloride electrode and uses a stable new electrochemical chlorination method to replace the gas-phase chlorination reaction, enabling the preparation of large-capacity single-cell batteries with different capacities.
[0006] To achieve the above objectives, the present invention adopts the following technical solution:
[0007] A method for preparing a metal / metal chloride electrode includes the following steps:
[0008] Step 1: Stack the active metal electrode B and the foam metal A in a cross manner to form an electrode. Place the electrode into an electrolytic cell and add molten salt as an electrolyte to the electrolytic cell. The main salt in the molten salt is a chloride containing metal B cations.
[0009] Step 2: Using active metal sheet B as the cathode and foamed metal A as the anode, electrolysis is performed by applying a constant current or voltage. After electrolysis, AC1 is generated on the surface of foamed metal A. x Membrane, yielding A / ACl x electrode;
[0010] Step 3: After electrolysis, the A / ACl... x The electrode is removed from the electrolytic cell while it is in a molten state.
[0011] Furthermore, prior to step 1, the foam metal A is cut, cleaned, and dried.
[0012] Furthermore, in step 1, the cross-stacking is: multiple units are stacked together, each unit including a cathode active metal sheet B, a first non-conductive grid, a foam metal A and a second non-conductive grid stacked in sequence, and a last layer of active metal sheet B is stacked to obtain an electrode.
[0013] Furthermore, in step 1, the foam metal A is a metallic element with a higher potential than the active metal sheet B.
[0014] Furthermore, in step 1, foam metal A is foam nickel or foam iron.
[0015] Furthermore, in step 2, a constant current density of 0.4 mA-2.0 mA / cm² is applied during electrolysis. 2 Or a constant voltage of 1.2-1.4V.
[0016] Furthermore, in steps 2 and 3, the operation is carried out in an inert atmosphere glove box.
[0017] Furthermore, in step 2, the electrolysis operating temperature is higher than the melting point of the electrolyte.
[0018] A metal / metal chloride electrode, prepared by the above method, comprises metal A and a chloride film of A covering metal A.
[0019] A metal-graphite molten salt battery, wherein the negative electrode is a metal / metal chloride electrode prepared by the above method.
[0020] Compared with the prior art, the present invention has at least the following beneficial technical effects:
[0021] 1) The electrode preparation process of this invention is simpler and more controllable, improving the consistency of metal / metal chloride electrodes. Currently, a large number of multi-module batteries face the problem of battery consistency, mainly due to uncontrollable factors in the electrode manufacturing process. Poor electrode consistency leads to lagging batteries, affecting the capacity output of the entire module. The negative electrode prepared by the method provided in this invention allows for precise control of the electrolysis current density, electrolysis time, and electrolysis potential using a potentiostat. Furthermore, the formed chloride layer and surface solid film are uniformly distributed, ensuring good electrode consistency. It can be used as a stable negative electrode for metal-graphite batteries.
[0022] 2) The preparation method of this invention avoids the complex pre- and post-treatment processes encountered in the conventional preparation of metal / metal chloride anodes. Due to the use of a molten salt electrolysis process, impurities and rust on the electrode surface are incorporated into the electrolyte under high potential conditions, eliminating the need for complex rust removal operations. The preparation process only requires a stable constant current or voltage source, avoiding the use of highly polluting and corrosive chemicals. The chloride-containing substance formed on the electrode surface after electrolysis does not contain complex products such as moisture, thus eliminating the need for subsequent dehydration annealing in an argon atmosphere.
[0023] 3) This method for preparing the negative electrode has lower production costs. First, the electrolysis process mainly involves converting electrical energy into chemical energy, and the required electrical energy can be directly generated by low-voltage DC or constant low voltage from new energy power generation devices. Second, the molten salt electrolyte used in the electrolysis process can be reused in subsequent electrolysis, making it suitable for continuous electrolysis of multiple batches of electrodes.
[0024] The metal / metal chloride anode of this invention can directly generate metal chlorides through electrolytic oxidation in a molten salt environment, avoiding heterogeneous impurities introduced by conventional preparation processes, thereby improving the cycle stability of the battery. Attached Figure Description
[0025] Figure 1a The cycling performance curve of the negative electrode obtained in Example 1 of this invention in a nickel-graphite battery;
[0026] Figure 1b The voltage curve of the negative electrode in a nickel-graphite battery obtained in Example 1 of the present invention is shown.
[0027] Figure 2a The cycling performance curve of the negative electrode obtained in Example 2 of this invention in a nickel-graphite battery;
[0028] Figure 2b The voltage curve of the negative electrode in a nickel-graphite battery obtained in Example 2 of this invention;
[0029] Figure 3a The cycling performance curve of the negative electrode obtained in Example 3 of this invention in an iron-graphite battery;
[0030] Figure 3b The voltage curve of the negative electrode in the iron-graphite battery obtained in Example 3 of the present invention is shown.
[0031] Figure 4a The cycling performance curve of the negative electrode obtained in Example 4 of this invention in an iron-graphite battery;
[0032] Figure 4b The voltage curve of the negative electrode in the iron-graphite battery obtained in Example 4 of the present invention is shown.
[0033] Figure 5a The cycling performance curve of the negative electrode obtained in Example 5 of this invention in an iron-graphite battery;
[0034] Figure 5b The voltage curve of the negative electrode in the iron-graphite battery obtained in Example 5 of the present invention is shown.
[0035] Figure 6a The cycling performance curve of the negative electrode obtained in Example 6 of this invention in an iron-graphite battery;
[0036] Figure 6b The voltage curve of the negative electrode in the iron-graphite battery obtained in Example 6 of the present invention;
[0037] Figure 7a An optical image of a rusted foam iron electrode used in Embodiment 6 of the present invention;
[0038] Figure 7b An optical image of the negative electrode surface obtained in Embodiment 6 of the present invention;
[0039] Figure 8a The cycling performance curve of the negative electrode obtained in Comparative Example 1 in a nickel-graphite battery is shown.
[0040] Figure 8b The voltage curve of the negative electrode in the nickel-graphite battery obtained in Comparative Example 1 is shown.
[0041] Figure 9a Cycling performance curves of the negative electrode obtained in Comparative Example 2 in an iron-graphite battery;
[0042] Figure 9b The cycle performance voltage curve of the negative electrode obtained in Comparative Example 2 in an iron-graphite battery;
[0043] Figure 10a SEM images of the original foamed iron and the foamed iron negative electrode obtained in Comparative Example 2;
[0044] Figure 10b The XRD patterns of the original foamed iron and the negative electrode obtained from Comparative Example 2 are shown.
[0045] Figure 11a Here are the SEM and EDS images of the foamed iron negative electrode obtained in Example 4;
[0046] Figure 11b The Raman spectra of the negative electrodes obtained in Examples 4 and 5;
[0047] Figure 12a SEM image of the original nickel foam;
[0048] Figure 12b The image shown is the SEM image of the negative electrode obtained in Comparative Example 1.
[0049] Figure 12c The image shows the SEM image of the negative electrode obtained in Example 2.
[0050] Figure 13 This describes the stacking method of the cathode and anode electrodes in the electrolysis process of this invention.
[0051] In the attached diagram: 1. Active metal sheet B; 2. First non-conductive grid; 3. Foam metal A; 4. Second non-conductive grid. Detailed Implementation
[0052] To make the objectives and technical solutions of this invention clearer and easier to understand, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. The specific embodiments described herein are for illustrative purposes only and are not intended to limit the invention.
[0053] A metal / metal chloride (N / NCl) x The method for preparing the negative electrode includes the following steps:
[0054] Step 1: Cut, clean, and dry the foam metal A, then sonicate it in pure water and anhydrous ethanol for 15 minutes each, and then dry it.
[0055] Step 2: Mix the active metal sheet B1 and the foam metal A3 according to... Figure 13The electrodes are assembled sequentially, with multiple units stacked together. Each unit includes a cathode active metal sheet B1, a first non-conductive grid 2, a foam metal A3, and a second non-conductive grid 4 stacked sequentially. An active metal sheet B is stacked on the outside of the last unit to obtain the electrode. The stacked electrode is then placed into an electrolytic cell, and an inorganic molten salt is added as the electrolyte. All of these are chloride molten salts: a mixture of NaCl, AlCl3, ZnCl2, KCl, and LiCl.
[0056] Step 3: Using the active metal sheet B as the cathode and the foamed metal A as the anode, electrolysis is performed by applying a constant current or potential, and the current density is controlled within the range of 0.4 mA-2.0 mA / cm². 2 Or, with a constant potential range of 1.2-1.4V, AC1 will be generated on the surface of foam metal A after the electrolysis process. x To obtain A / ACl x electrode;
[0057] Step 4: After electrolysis, the A / ACl... x The electrode was removed from the electrolytic cell in a molten state and the A / ACl was drained. x After the molten salt electrolyte is removed from the electrode surface, the molten salt electrolyte is cleaned with DME.
[0058] Furthermore, in step one, foam metal A is foam nickel, and iron is a metal element with an equipotential higher than that of the cathode.
[0059] Furthermore, in step two, the active metal sheet B is a metal such as zinc or aluminum with an electrode potential lower than that of electrode A. The main salt in the corresponding molten salt electrolyte is a chloride containing metal B cations, and the molar proportion of the main salt in the molten salt electrolyte is higher than 40%. The main function of adding the remaining chlorides is to lower the melting point of the molten salt.
[0060] Furthermore, steps two through four must be performed in an inert atmosphere glove box, and the electrolysis operating temperature must match the melting point of the inorganic electrolyte, generally 20°C or more above its melting point.
[0061] The A / ACl prepared by the above method x Electrode, A / ACl x The electrode consists of foamed metal A and an Al group wrapped around foamed metal A. x membrane.
[0062] The metal / metal chloride anode prepared by the above method is used in metal-graphite molten salt batteries.
[0063] Metal-graphite molten salt battery, the negative electrode of which is A / ACl obtained by the above preparation method. x electrode.
[0064] An assembly method for a metal-graphite molten salt battery includes the following seven steps:
[0065] S1, A / ACl prepared by the above method x The electrode serves as the negative electrode of the battery and is welded using ultrasonic welding on an A / ACl substrate. x Metal nickel tabs are welded onto the electrodes.
[0066] S2. Use the graphite positive electrode (53mm*55mm in size) as the positive electrode of the battery. Cut the graphite positive electrode according to the area of the negative electrode, clean the graphite positive electrode with ethanol, and finally dry it.
[0067] S3. Use a metal molybdenum sheet (53mm*55mm) as the positive current collector. After cutting and leaving the tabs, sand it with sandpaper, clean it with water and ethanol, and dry it.
[0068] S4. Following the repeating unit of positive electrode, separator, and negative electrode, place 4 pieces of A / ACl... x The negative electrode and five graphite positive electrode sheets are stacked to form a battery cell, which is then finally installed in a polytetrafluoroethylene battery casing to ensure that the positive and negative electrode tabs are combined and led out.
[0069] S5. Add sufficient amount of melted inorganic molten salt electrolyte to the polytetrafluoroethylene battery casing to ensure that the battery cell is fully wetted.
[0070] S6. After letting the battery stand for more than 3 hours, start the test.
[0071] Furthermore, step S5 uses a mixture of molten salt electrolytes such as AlCl3, NaCl, and LiCl.
[0072] Furthermore, steps S2-S6 must be performed in a glove box filled with inert gas or in a low-oxygen environment.
[0073] The method provided by this invention can realize the preparation and large-scale production of metal-graphite battery anodes with stable electrochemical performance, low cost, and large capacity.
[0074] The following are relevant embodiments for verifying the technology described in this invention:
[0075] Example 1
[0076] S1. Cut and clean the foamed nickel metal (50mm*52mm in size). First, ultrasonically treat with pure water for 15 minutes and rinse once. Then, ultrasonically treat with anhydrous ethanol for 15 minutes. After rinsing, dry in a forced-air drying oven until completely dry.
[0077] S2. Using metallic zinc as the electrolytic cathode and cleaned foamed nickel as the anode, the two are stacked together and separated by porous polytetrafluoroethylene before being placed in an electrolytic cell.
[0078] S3. Add the molten electrolyte salt (ZnCl2:NaCl:LiCl molar ratio of 4:3:3) to the above electrolytic cell and keep the temperature constant at 180℃.
[0079] S4. Electrolysis is performed using a constant current, with the current density adjusted to 1.0 mA / cm². 2 The cutoff voltage is controlled at 1.2V until the electrolysis is completed.
[0080] S5. After the electrolysis process is completed, a Ni / NiCl2 negative electrode is obtained. The obtained Ni / NiCl2 negative electrode is used to assemble a nickel-graphite battery according to the assembly steps of a metal-graphite molten salt battery described above, and a constant current test is performed.
[0081] Example 2
[0082] S1. Clean the foamed nickel metal (same size as above). First, ultrasonically treat with pure water for 15 minutes and rinse once. Then, ultrasonically treat with anhydrous ethanol for 15 minutes. After rinsing, dry in a forced-air drying oven until completely dry.
[0083] S2. Metallic Al is used as the electrolytic cathode, and cleaned foamed iron is used as the anode. After stacking, they are separated by porous polytetrafluoroethylene and placed in the electrolytic cell.
[0084] S3. Add the molten electrolyte salt (AlCl3:NaCl:LiCl molar ratio of 2:1:1) to the above electrolytic cell and keep the temperature constant at 130℃.
[0085] S4. Electrolysis is performed using a constant current, with the current density adjusted to 1.0 mA / cm². 2 The control cutoff voltage is 1.2V.
[0086] S5. After the electrolysis process is completed, a Ni / NiCl2 negative electrode is obtained. The obtained Ni / NiCl2 electrode is then assembled into a nickel-graphite battery according to the steps in the specific implementation method, and a constant current test is performed.
[0087] Example 3
[0088] S1. Clean the foamed iron metal (same size as above). First, ultrasonically treat with pure water for 15 minutes and rinse once. Then, ultrasonically treat with anhydrous ethanol for 15 minutes. After rinsing, dry in a forced-air drying oven until completely dry.
[0089] S2. Metallic Zn is used as the electrolytic cathode, and cleaned foamed iron is used as the anode. After stacking, they are separated by porous polytetrafluoroethylene and placed in the electrolytic cell.
[0090] S3. Add the molten electrolyte salt (ZnCl2:NaCl:LiCl molar ratio of 4:3:3) to the above electrolytic cell and keep the temperature constant at 180℃.
[0091] S4. Electrolysis is performed using a constant current, with the current density adjusted to 0.4 mA / cm². 2 The control cutoff voltage is 1.4V.
[0092] S5. After the electrolysis process is completed, Fe / FeCl2 negative electrode is obtained. The obtained Fe / FeCl2 negative electrode is used to assemble an iron-graphite battery according to the steps in the specific implementation method, and constant current test is performed.
[0093] Example 4
[0094] S1. Clean the foamed iron metal (same size as above). First, ultrasonically treat with pure water for 15 minutes and rinse once. Then, ultrasonically treat with anhydrous ethanol for 15 minutes. After rinsing, dry in a forced-air drying oven until completely dry.
[0095] S2. Metallic Al is used as the electrolytic cathode, and cleaned foamed iron is used as the anode. After stacking, they are separated by porous polytetrafluoroethylene and placed in the electrolytic cell.
[0096] S3. Add the molten electrolyte salt (AlCl3:NaCl:LiCl molar ratio of 2:1:1) to the above electrolytic cell and keep the temperature constant at 130℃.
[0097] S4. Electrolysis is performed using a constant current, with the current density adjusted to 1.0 mA / cm². 2 The control cutoff potential is 1.3V.
[0098] S5. After the electrolysis process is completed, Fe / FeCl2 negative electrode is obtained. The obtained Fe / FeCl2 electrode is assembled into an iron-graphite battery according to the steps in the specific implementation method, and constant current test is performed.
[0099] Example 5
[0100] S1. Clean the foamed iron metal of the same size. First, ultrasonically treat with pure water for 15 minutes and rinse once. Then, ultrasonically treat with anhydrous ethanol for 15 minutes. After rinsing, dry in a forced-air drying oven until completely dry.
[0101] S2. Metallic Al is used as the electrolytic cathode, and the cleaned foamed iron electrode is used as the anode. After stacking, the electrodes are separated by porous polytetrafluoroethylene and placed in the electrolytic cell.
[0102] S3. Add the molten electrolyte salt (AlCl3:NaCl:LiCl molar ratio of 2:1:1) to the above electrolytic cell and keep the temperature constant at 130℃.
[0103] S4. Electrolysis is performed using a constant potential process, with the potential fixed at 1.2V and the cutoff current controlled at 0.1A.
[0104] S5. After the electrolysis process is completed, Fe / FeCl2 negative electrode is obtained. The obtained Fe / FeCl2 electrode is assembled into an iron-graphite battery according to the steps in the specific implementation method, and constant current test is performed.
[0105] Example 6
[0106] The preparation process of this embodiment is the same as that of embodiment 4, except that the foamed iron used in step 1 has rust on its surface, and the electrolysis current density is controlled at 2.0 mA / cm². 2 The assembled iron-graphite battery has 3 positive electrodes and 2 negative electrodes. The preparation process of other electrodes and the battery assembly process are the same as in Example 4.
[0107] Comparative Example 1
[0108] S1. Cut the foamed nickel metal (52mm*54mm in size) and clean it. First, ultrasonically treat it with pure water for 15 minutes and rinse it once. Then, ultrasonically treat it with anhydrous ethanol for 15 minutes. After rinsing, dry it in a forced-air drying oven until it is completely dry.
[0109] S2. Place the above electrodes in a sealed container and react for 6 hours using an Ar / HCl atmosphere and hydrogen chloride gas from concentrated hydrochloric acid vapor.
[0110] S3. Place the chemically chlorinated electrode in a resistance furnace and remove the water of crystallization at 600°C in an argon atmosphere.
[0111] S5. After the dehydration process is completed, the obtained Ni / NiCl2 electrode is assembled into a nickel-graphite battery according to the steps in the specific implementation method, and a constant current test is performed.
[0112] Comparative Example 2
[0113] S1. Cut and clean the foamed iron. First, ultrasonically treat it with pure water for 15 minutes and rinse it once. Then, ultrasonically treat it with anhydrous ethanol for 15 minutes, rinse it, and then dry it thoroughly in a forced-air drying oven.
[0114] S2. Place the above electrodes in a sealed container and react for 6 hours using an Ar / HCl atmosphere and hydrogen chloride gas from concentrated hydrochloric acid vapor.
[0115] S3. Place the chemically chlorinated electrode in a resistance furnace and remove the water of crystallization at 600°C in an argon atmosphere.
[0116] S5. After the dehydration process is completed, the obtained Fe / FeCl2 electrode is assembled into an iron-graphite battery according to the steps in the specific implementation method, and a constant current test is performed.
[0117] The A / ACl2 anode prepared according to this invention is mainly used in metal-graphite batteries. Firstly, the metal-graphite battery uses a metal chloride as the anode, graphite as the cathode, and an inorganic molten salt as the electrolyte. The battery is assembled in a fully discharged state, where the graphite is in an unintercalated anionic state, and the anode is in a metal chloride state. After the first charge, anions intercalate into the graphite cathode, and the corresponding metal chloride in the anode is reduced to elemental metal. Subsequent cycles mainly involve repeated intercalation / deintercalation reactions and redox processes. For the A / ACl2 anode, different preparation methods correspond to different electrode performance and full-cell performance. Examples 1-5 of this invention verify the electrochemical performance of anodes prepared by different processes in metal-graphite batteries, while Comparative Examples 1-2 provide the battery performance of anodes prepared by chemical chlorination in full-cell batteries. Simultaneously, physical characterization methods such as SEM, EDS, XRD, and Raman spectroscopy fully reveal the differences in the active materials formed on the electrode surface by these two preparation methods.
[0118] first, Figure 1a , Figure 1b , Figure 2a and Figure 2b When using nickel foam as the anode material for electrolysis, the electrochemical performance of the nickel-graphite battery anodes prepared in Examples 1-2 is as follows: the electrochemical window of the nickel-graphite battery is 1.5-2.0V. The Ni / NiCl2 electrode obtained in Example 1 exhibits a full-cell capacity of 57mAh in a 20mA constant current charge-discharge test in a nickel-graphite battery. The corresponding voltage curves show a clear positive electrode insertion / deintercalation reaction plateau at 1.9V during charging and 1.85V and 1.75V during discharging. Example 2, by changing the electrolyte and electrolytic cathode, can also prepare a nickel anode, and its battery performance is as follows. Figure 2a and Figure 2b As shown, the battery capacity is 40mAh under a current density of 10mA, and the corresponding voltage curve indicates that it exhibits a more pronounced voltage plateau at similar potentials. Comparative Example 1 uses a Ni / NiCl2 anode prepared by gas-phase chemical chlorination (…). Figure 8a , Figure 8bUnder the same current density conditions, the battery capacity was only 27mAh, significantly lower than that of the electrochemical chlorination method used in this invention. The voltage curve of the chemical chlorination electrode also showed a lower voltage plateau (<1.6V) during discharge, indicating that the chemical chlorination electrode exhibited the highest polarization, leading to a rapid voltage drop during use. Example 3 involved preparing a Fe / FeCl2 negative electrode using foamed iron as the raw material through a constant current process. The voltage window of the iron-graphite battery was 0.8-1.8V. The Ni / NiCl2 negative electrode prepared using a zinc electrode as the electrolytic cathode showed a slight capacity increase in the iron-graphite battery, with a decrease in coulombic efficiency in the later stages of cycling. After 100 cycles, the battery capacity was 88mAh. The corresponding voltage curves showed that the battery mainly had a charging plateau of 1.5V and discharge plateaus of 1.4V and 1.1V during charging, and the curves corresponding to different cycle numbers had good overlap, indicating that the Fe / FeCl2 negative electrode prepared with foamed iron also had good electrochemical reversibility in the full cell. Figure 4a To replace the cathode with metallic aluminum and the electrolyte with ternary aluminum molten salt, a 160mAh-level iron-graphite battery was prepared using a constant current process with Fe / FeCl2 anode assembly. At the same current density of 40mA, the battery released 166mAh of discharge capacity after 100 cycles, with a coulombic efficiency close to 96%. According to the corresponding voltage curves, the potential plateau during the charge-discharge process was basically consistent with that of Example 3, indicating that the Fe / FeCl2 anodes prepared under these two electrolysis conditions have the same surface state. Regarding the initial electrode surface state, this electrochemical chlorination method also showed high tolerance to corroded foam metal. Example 6 demonstrated that the corrosion present on the electrode surface after cleaning in step 1 did not affect the subsequent electrode reaction. After a high current density electrolysis process, the electrode still had a discharge capacity of 33mAh after 100 cycles in the iron-graphite battery, and the charge-discharge curve was basically the same as that of Example 4. The Fe / FeCl2 anode surface obtained after the electrolysis reaction darkened in color (…). Figure 7a and Figure 7bApart from the solidified electrolyte, there were no significant differences. This is mainly because high-valence compound impurities on the electrode surface are more easily incorporated into the electrolyte during electrolysis, and the newly generated ferrous chloride makes the electrode surface more homogeneous. Meanwhile, to adapt to different electrolysis conditions, the method of preparing Fe / FeCl2 anodes using a constant potential process was further verified. According to Example 5, the Fe / FeCl2 anode prepared using a 1.2V constant potential process exhibited the same electrochemical behavior in an iron-graphite battery. The corresponding battery, under the same current density, could release a discharge capacity of 67mAh after 100 cycles, with a coulombic efficiency of 97%, proving that the Fe / FeCl2 anode prepared by this electrochemical chlorination process has the same surface products and can cycle stably in a full cell. Compared with the Fe / FeCl2 anode prepared by chemical chlorination (Comparative Example 2), the battery exhibited a lower voltage plateau of 1.35V and 1.0V during discharge, indicating that the polarization phenomenon during discharge was greater than that of the electrochemical chlorination electrode. Furthermore, the battery showed significant discharge capacity decay at a current density of 40mA. Figure 9a , Figure 9b The low coulombic efficiency (91%) indicates that the Fe / FeCl2 anode prepared by chemical chlorination has poor cycle stability and reversibility.
[0119] Meanwhile, in order to demonstrate the characteristics of the active substances formed on the electrode surface during this electrochemical chlorination process, Figure 10a , Figure 10b , Figure 11a and Figure 11b SEM images and corresponding XRD patterns of the original foamed iron electrode and the chemically chlorinated foamed iron electrode are shown respectively. It can be found that ferrous chloride formed by the displacement reaction between hydrochloric acid vapor and elemental iron during the gas-phase chemical chlorination process is an irregular columnar crystal with obvious crystal morphology characteristics. XRD confirms that this crystal is anhydrous ferrous chloride and has good crystallinity. Figure 11a and Figure 11b SEM and EDS images show the surface of the iron electrode after electrochemical chlorination in this invention. An irregular surface solid film and spherical particles were observed. Raman spectroscopy confirmed the presence of low-crystallinity ferrous chloride, which is speculated to be related to the electrolytic current density and its dissolution process in the electrolyte. Compared to the high-crystallinity product formed by gas-phase chemical chlorination, this low-crystallinity ferrous chloride exhibits faster redox kinetics and higher electrode capacity in the electrochemical reaction. Regarding the surface products of the nickel electrode... Figure 12a , Figure 12b and Figure 12cThe surface morphologies of the original nickel foam electrode, the chemically chlorinated nickel foam electrode, and the electrochemically chlorinated nickel foam electrode are shown respectively. It can be found that their surface structures exhibit similar patterns to those of the iron electrode mentioned above. The chemical chlorination process tends to form crystalline chlorides with high crystallinity, while the electrochemical chlorination in this invention tends to form solid film chlorides with low crystallinity. Electrochemical performance test results show that the latter has lower electrochemical polarization and better electrochemical performance in metal-graphite batteries. At the same time, the research results of this type of electrode also demonstrate the reliability of this electrochemical chlorination preparation technology in the production of metal / metal chloride electrodes.
[0120] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.
Claims
1. A method for preparing a metal / metal chloride electrode, characterized in that, Includes the following steps: Step 1: Stack the active metal electrode B and the foam metal A in a cross manner to form an electrode. Place the electrode into an electrolytic cell and add molten salt as an electrolyte to the electrolytic cell. The main salt in the molten salt is a chloride containing metal B cations. Step 2: Using active metal sheet B as the cathode and foamed metal A as the anode, electrolysis is performed by applying a constant current or voltage. After electrolysis, AC1 is generated on the surface of foamed metal A. x Membrane, yielding A / ACl x electrode; Step 3: After electrolysis, the A / ACl... x The electrodes are removed from the electrolytic cell while still in a molten state. In step 1, foam metal A is a metallic element with a higher potential than active metal sheet B; In step 1, foam metal A is foam nickel or foam iron.
2. The method for preparing a metal / metal chloride electrode according to claim 1, characterized in that, Before step 1, the foam metal A is cut, cleaned, and dried.
3. The method for preparing a metal / metal chloride electrode according to claim 1, characterized in that, In step 1, the cross-stacking is: multiple units are stacked together, each unit including a cathode active metal sheet B, a first non-conductive grid, foam metal A and a second non-conductive grid stacked in sequence, and a single active metal sheet B is stacked as the last layer to obtain an electrode.
4. The method for preparing a metal / metal chloride electrode according to claim 1, characterized in that, In step 2, a constant current density of 0.4 mA-2.0 mA / cm² is applied during electrolysis. 2 Or a constant voltage of 1.2-1.4V.
5. The method for preparing a metal / metal chloride electrode according to claim 1, characterized in that, In steps 2 and 3, the operation is carried out in an inert atmosphere glove box.
6. The method for preparing a metal / metal chloride electrode according to claim 1, characterized in that, In step 2, the electrolysis operating temperature is higher than the electrolyte melting point.
7. A metal / metal chloride electrode, characterized in that, Prepared using the method of claim 1, comprising metal A and a chloride film of A covering metal A.
8. A metal-graphite molten salt battery, characterized in that, The negative electrode is a metal / metal chloride electrode prepared by the method of claim 1.
Citation Information
Patent Citations
Molten salt battery-based thermoelectric integrated energy storage system and energy storage method