Inorganic solid-state electrolyte and method for preparing the same

Inorganic solid electrolytes were prepared by using doped tin-based perovskite CsSnCl₃, which solved the problems of low ionic conductivity and structural instability of chloride-ion batteries at room temperature, and realized high energy density and electrochemical stability of chloride-ion batteries.

CN117638207BActive Publication Date: 2026-11-24NANJING TECH UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311447251.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-02
Publication Date
2026-11-24
Estimated Expiration
2043-11-02

AI Technical Summary

Technical Problem

The solid electrolytes in existing chloride-ion batteries have low ionic conductivity at room temperature, unstable structure, and are easily soluble in liquid electrolytes, leading to capacity decay and battery failure.

Method used

The inorganic solid electrolyte is prepared by ball milling using element-doped tin-based perovskite CsSnCl₃. The doping elements include lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron, forming a stable cubic phase structure, which improves ionic conductivity and enhances electrochemical stability.

Benefits of technology

It achieves high ionic conductivity and a wide electrochemical stability window, solves the problem of chloride-ion batteries dissolving in liquid electrolytes, and improves the energy density and electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004527791500000011
    Figure HDA0004527791500000011
  • Figure HDA0004527791500000012
    Figure HDA0004527791500000012
  • Figure HDA0004527791500000021
    Figure HDA0004527791500000021
Patent Text Reader

Abstract

This invention provides an inorganic solid electrolyte and its preparation method. The electrolyte is characterized by being an element-doped tin-based perovskite (CsSnCl3), wherein the doping element is one of lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron; the molar percentage of the doping element is 0.5%–50%. This electrolyte is prepared by mechanical ball milling, directly yielding a stable cubic phase structure. The electrolyte of this invention exhibits a wide electrochemical stability window, high ionic conductivity, and excellent low-temperature and high-humidity stability. This solves a key problem for developing high-voltage, high-energy-density chloride-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of chloride-ion battery technology, and more specifically to an inorganic solid electrolyte and its preparation method. Background Technology

[0002] Inorganic solid materials, such as oxides, sulfides, and halides, capable of conducting alkali metal ions, have been extensively explored as solid electrolytes for high-energy-density, safe solid-state rechargeable batteries based on cation transport. Recent research interest has also focused on anionic solid electrolytes, which utilize anion carriers such as hydride ions and halide ions (F...). - Cl - , Br - , or I - Chloride can be used to realize another form of rechargeable battery. The use of chloride ion carriers has demonstrated the advantages of chloride batteries, such as abundant material resources, eco-friendliness, and high energy density electrode systems. However, some excellent chloride electrode materials are soluble in liquid electrolytes, exhibiting poor compatibility with liquid electrolytes, leading to severe capacity decay and battery failure. In addition to structural adjustments to liquid electrolytes, the use of high-performance solid-state electrolytes holds promise for solving these problems. However, chloride ion conductors with ideal chemical and electrochemical stability, stable phase structure, and high ionic conductivity at room temperature are rare.

[0003] Derrington et al., in their report published in the Journal of Solid State Chemistry, Volume 15, page 171, have reported that some metal chlorides (such as lead chloride, stannous chloride, and barium chloride) and metal oxychlorides (such as lanthanum oxychloride) have exhibited chloride ion conductor properties. However, high temperatures above 500 K are required to obtain approximately 10 -5 Scm -1 The ionic conductivity; RyoSakamoto et al. reported in the journal Chem ElectroChem, Volume 8, page 4441, using potassium-doped lead chloride (Pb) 0.98 K 0.02 Cl 1.98 Chloride ion conduction can be achieved at a low temperature of approximately 333 K. Wu Bing et al., in *Energy & Environmental Materials*, reported that the preparation of [Al(DMSO)6]Cl3 organometallic crystals via the coordination reaction of aluminum trichloride with dimethyl sulfoxide further lowered the temperature to 298 K. However, these metal chloride conductors may undergo chemical or electrochemical redox reactions within a narrow electrochemical window. Furthermore, unlike metal fluorides which exhibit good stability under environmental conditions, metal chlorides are sensitive to moisture, which can cause anhydrous chlorides to decompose into hydrates, thereby losing their chloride ion conductivity.

[0004] Another type of inorganic chloride ion conductor is the perovskite-type chloride (such as tin halide perovskite CsSnCl3), which can be prepared by reacting cesium chloride with stannous chloride. At 313 K, cubic tin halide perovskite CsSnCl3, with a suitable band gap (approximately 3.0 eV), exhibits a conductivity of 10-1. -4 S cm -1 That's all. However, this material loses its cubic structure at around room temperature or when in contact with moisture, forming an insulating monoclinic phase, indicating poor structural stability and still failing to meet the requirements for use. Summary of the Invention

[0005] The purpose of this invention is to address the shortcomings of existing technologies by providing an inorganic solid-state electrolyte for use in chloride-ion batteries, which exhibits good ionic conductivity and high electrochemical stability. Another objective of this invention is to provide a method for preparing the aforementioned inorganic solid-state electrolyte. A further objective is to construct a solid-state rechargeable chloride-ion battery using the aforementioned inorganic solid-state electrolyte.

[0006] The first aspect of the present invention is to provide an inorganic solid electrolyte for use in chloride-ion batteries, characterized in that the electrolyte is composed of element-doped halogen tin-based perovskite CsSnCl3, wherein the doping element includes one of lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron.

[0007] Preferably, the molar percentage of one of the doped elements, lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron, is 0.5% to 50%.

[0008] The present invention also provides a method for preparing the above-mentioned inorganic solid electrolyte, comprising the following steps: adding the chloride of the doped element into a ball mill jar and ball milling under an inert atmosphere for 0.5 to 24 hours to directly obtain the element-doped cubic tin halide perovskite CsSnCl3 inorganic solid electrolyte.

[0009] The preferred doping element is a chlorine compound such as lanthanum chloride, antimony chloride, bismuth chloride, vanadium chloride, niobium chloride, neodymium chloride, or ferric chloride.

[0010] The preferred ball-to-material mass ratio for ball milling is 5–50:1, and the rotation speed is 300–500 rpm. The preferred inert atmosphere is nitrogen or argon, more preferably argon.

[0011] The all-solid-state rechargeable chloride-ion battery constructed from the aforementioned inorganic solid-state electrolyte is characterized by assembling the inorganic solid-state electrolyte with a positive electrode material and a negative electrode material; wherein the positive electrode material is a metal chloride, a metal chlorine oxide, or a chlorinated organic compound, and the negative electrode material is lithium metal, magnesium, or calcium, or a chlorinated organic compound.

[0012] Preferably, the metal chloride is vanadium chloride, chromium chloride, manganese chloride, ferric chloride, cobalt chloride, nickel chloride, copper chloride, tin chloride, or bismuth chloride; the metal chlorine oxide is ferric chloride, bismuth chloride, antimony chloride, vanadium chloride, niobium chloride, or molybdenum chloride; and the chlorine-containing organic compound is polyvioletin, polyaniline, or polypyrrole.

[0013] As can be seen from the above solutions, the significant advantages of the inorganic solid electrolyte proposed in this invention for use in chloride-ion batteries are:

[0014] The inorganic solid electrolyte of this invention uses tin-halogenated perovskite CsSnCl3 as a matrix and is doped with one of the following elements: lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron. When the doping element is bismuth and the doping ratio is 0.5% to 50%, a stable cubic phase structure can be obtained, and the room temperature ionic conductivity is greater than 10. -5 S cm -1 It has high ionic conductivity, low electronic conductivity, and excellent chloride ion conduction capability, and can be successfully applied to chloride ion batteries.

[0015] The rechargeable chloride-ion battery constructed using the above-mentioned inorganic solid electrolyte can solve the desolvation and side reactions that exist when using liquid electrolyte in chloride-ion batteries, thus promising the application of high-energy-density metal chloride cathodes and high-capacity magnesium anodes. Attached Figure Description

[0016] Figure 1 These are the X-ray diffraction patterns of the element-doped tin halide perovskite CsSnCl3 inorganic solid electrolytes prepared in comparative examples and Examples 1-7 of this invention.

[0017] Figure 2 This is a scanning electron microscope image of the bismuth-doped halotin-based perovskite CsSnCl3 inorganic solid electrolyte in Example 3 of the present invention.

[0018] Figure 3 yes Figure 2 The corresponding elemental mapping image of the energy spectrum.

[0019] Figure 4 Arenius diagrams of element-doped tin-based perovskite CsSnCl3 inorganic solid electrolytes prepared in Comparative Examples and Examples 1-7.

[0020] Figure 5 The electronic conductivity diagrams are for the element-doped tin halide perovskite CsSnCl3 inorganic solid electrolytes prepared in Examples 1-7.

[0021] Figure 6 Linear scan voltammetry of the bismuth-doped halotin-based perovskite CsSnCl3 inorganic solid electrolyte in Example 3;

[0022] Figure 7 The charge-discharge curves are shown for a chloride-ion battery constructed using the bismuth-doped halotin-based perovskite CsSnCl3 inorganic solid electrolyte from Example 3.

[0023] Figure 8 The charge-discharge curves are shown for a chloride-ion battery constructed using the vanadium-doped halogenated tin-based perovskite CsSnCl3 inorganic solid electrolyte from Example 4.

[0024] Figure 9 The charge-discharge curves are shown for a chloride-ion battery constructed using the iron-doped halogenated tin-based perovskite CsSnCl3 inorganic solid electrolyte from Example 7. Detailed Implementation

[0025] To better understand the technical content of the present invention, specific embodiments are described below in conjunction with the accompanying drawings.

[0026] Various aspects of the invention are described in this disclosure with reference to the accompanying drawings, in which numerous illustrative embodiments are shown. The embodiments of this disclosure are not necessarily intended to encompass all aspects of the invention. It should be understood that the various concepts and embodiments described above, as well as those described below in more detail, can be implemented in any of a number of ways.

[0027] The present invention aims to provide an inorganic solid electrolyte for use in chloride-ion batteries, which has a wide electrochemical stability window, high ionic conductivity and excellent chloride ion conduction capability.

[0028] The features of embodiments of the present invention will be listed and described below.

[0029] In one embodiment of the present invention, an inorganic solid electrolyte for use in chloride-ion batteries is proposed, the electrolyte comprising element-doped tin-based perovskite CsSnCl3, the electrolyte being prepared by mechanical ball milling.

[0030] The aforementioned doping elements are mainly doped into the tin positions of the tin-containing tin-based perovskite CsSnCl3, replacing tin with one of the following elements: lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron. These elements not only stabilize the cubic phase structure of the perovskite but also improve the ionic conductivity to some extent.

[0031] In an optional embodiment, the proportion of the dopant element is 0.5% to 50%.

[0032] Another embodiment of the present invention relates to a method for preparing the aforementioned inorganic solid electrolyte for use in chloride-ion batteries, comprising the following steps:

[0033] Cesium chloride, stannous chloride, and the chloride of the doped element are mixed in a glove box and poured into a ball mill jar. The mixture is then ball-milled in a planetary ball mill under an inert atmosphere. After the reaction, a cubic phase inorganic solid electrolyte doped with lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron is directly obtained. The reaction time is generally controlled between 0.5 and 24 hours. The preferred chloride compounds of the doped element are lanthanum chloride, antimony chloride, bismuth chloride, vanadium chloride, niobium chloride, neodymium chloride, or iron chloride.

[0034] In an optional embodiment, the doping ratio of lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron is 0.5% to 50%, the ball-to-material mass ratio of the ball mill is 5:1 to 50:1, and the ball milling speed is 300 to 500 rpm.

[0035] Other embodiments of the present invention involve chloride-ion batteries in which the electrolyte is the aforementioned inorganic solid electrolyte used in chloride-ion batteries. This electrolyte has a wide electrochemical stability window, high ionic conductivity and excellent chloride-ion conduction capability. Therefore, the chloride-ion battery has excellent electrochemical performance.

[0036] To facilitate better understanding, the present invention will be further illustrated below with several specific examples, but the materials and processing techniques are not limited thereto, and the content of the present invention is not limited thereto.

[0037] Comparative Example

[0038] In an argon-filled glove box, cesium chloride and stannous chloride were mixed in a 1:1 molar ratio and added to a 100 ml stainless steel ball mill jar. The ball-to-material mass ratio was 30:1, and the milling speed was 300 rpm. Under sealed conditions, the mixture was transferred to a planetary ball mill for milling reaction for 1 hour, yielding undoped tin halide perovskite CsSnCl3 electrolyte. Figure 1 and Figure 4 As shown, the undoped CsSnCl3 electrolyte is not a cubic phase, and its room temperature ionic conductivity is approximately 10. -10 S cm -1 Much less than 10 -5 S cm -1 .

[0039] Example 1

[0040] In an argon-filled glove box, cesium chloride, stannous chloride, and lanthanum chloride were mixed in a molar ratio of 1:0.95:0.05 and added to a 100ml stainless steel ball mill jar. The ball-to-material mass ratio was 30:1, and the milling speed was 500 rpm. Under sealed conditions, the mixture was transferred to a planetary ball mill for milling reaction, which lasted for 12 hours, directly yielding a lanthanum-doped cubic tin halide perovskite CsSnCl3 electrolyte. Figure 1 As shown, the XRD pattern matched successfully with the standard PDF card, confirming successful doping and direct acquisition of cubic CsSnCl3. Figure 4 As shown, the lanthanum-doped CsSnCl3 electrolyte has an ionic conductivity of 1.04 × 10⁻⁶. -4 Scm -1 It has high room temperature ionic conductivity; such as Figure 5 As shown in Figure a, the electronic conductivity is only 10. -9 Scm -1 The difference between its conductivity and ionic conductivity is five orders of magnitude, indicating that it is an ionic conductor rather than an electronic conductor.

[0041] Example 2

[0042] In an argon-filled glove box, cesium chloride, stannous chloride, and antimony chloride were mixed in a molar ratio of 1:0.7:0.3 and added to a 100ml stainless steel ball mill jar. The ball-to-material mass ratio was 5:1, and the milling speed was 400 rpm. Under sealed conditions, the mixture was transferred to a planetary ball mill for milling reaction, which lasted for 24 hours, directly yielding an antimony-doped cubic tin halide perovskite CsSnCl3 electrolyte. Figure 1 As shown, the XRD pattern matched the standard PDF card successfully, indicating successful doping and direct acquisition of cubic CsSnCl3. Figure 4 As shown, the antimony-doped CsSnCl3 electrolyte has an ionic conductivity of 1.41 × 10⁻⁶. -4 S cm -1 It has high room temperature ionic conductivity; such as Figure 5 As shown in Figure b, the electronic conductivity is also relatively small, much smaller than the ionic conductivity.

[0043] Example 3

[0044] In an argon-filled glove box, cesium chloride, stannous chloride, and bismuth chloride were mixed in a molar ratio of 1:0.95:0.05 and added to a 100 ml stainless steel ball mill jar. The ball-to-material mass ratio was 35:1, and the milling speed was 450 rpm. The mixture was then transferred to a planetary ball mill under sealed conditions for milling reaction for 0.5 hours, directly yielding a bismuth-doped cubic tin halide perovskite CsSnCl3 electrolyte.

[0045] The diffraction peaks of the bismuth-doped tin halolithic perovskite CsSnCl3 electrolyte prepared in this embodiment are consistent with the standard card (PDF No. 22-0200) of cubic tin halolithic perovskite CsSnCl3, and no other impurity diffraction peaks are observed, indicating that the prepared bismuth-doped tin halolithic perovskite CsSnCl3 electrolyte is free of impurities.

[0046] The bismuth-doped tin halooxide perovskite CsSnCl3 electrolyte prepared in this embodiment was subjected to field emission scanning electron microscopy (FET) analysis, and the results are as follows: Figure 2 As shown in the figure, the sample appears as irregular micron-sized particles, consistent with the characteristics of ball-milled samples; the corresponding energy dispersive spectroscopy elemental mapping image ( Figure 3 It can be seen that bismuth is uniformly doped in the tin-halogenated perovskite CsSnCl3.

[0047] like Figure 4 As shown, the bismuth-doped CsSnCl3 electrolyte has an ionic conductivity of 1.01 × 10⁻⁶. -4 S cm -1 It has high room temperature ionic conductivity; such as Figure 5 As shown in Figure c, the electronic conductivity is also relatively small, much smaller than the ionic conductivity.

[0048] The bismuth-doped tin-halogenated perovskite CsSnCl3 electrolyte prepared in this embodiment was packed into a blocking battery with stainless steel electrodes. The electrolyte was tested using linear sweep voltammetry on an electrochemical workstation at a temperature of 298 K and a scan rate of 5 mV / s. The results showed that the oxidation potential of the inorganic solid electrolyte was 2.35 V, the reduction potential was -2.48 V, and the electrochemical window was 4.83 V. The prepared inorganic solid electrolyte has a relatively wide electrochemical window. Figure 6 ).

[0049] A carbon current collector was prepared by mixing carbon nanotubes and graphene at a mass ratio of 9:1, and then pressed into a 12 mm radius disc inside a glove box. Copper chloride was dissolved in 0.5 mol / L PP... 14 Cl / PP 14 A mixed solution with a concentration of 0.05 g / mL was prepared in TFSI liquid electrolyte; 20 μL of the mixed solution was dropped onto a current collector to prepare a positive electrode. Using the positive electrode as the working electrode, lithium metal as the counter electrode and reference electrode, and the bismuth-doped tin halide perovskite CsSnCl3 solid prepared in this embodiment as the electrolyte, a blocking battery was assembled. Charge-discharge tests were performed using a Newway electrochemical workstation. Figure 7 As shown, the highest discharge specific capacity of the battery's positive electrode at a current density of 10 mA / g is 367 mAh / g.

[0050] Example 4

[0051] In an argon-filled glove box, cesium chloride, stannous chloride, and vanadium chloride were mixed in a molar ratio of 1:0.9:0.1 and added to a 100ml stainless steel ball mill jar. The ball-to-material mass ratio was 50:1, and the milling speed was 300 rpm. Under sealed conditions, the mixture was transferred to a planetary ball mill for milling reaction, which lasted for 12 hours, directly yielding a vanadium-doped cubic tin halide perovskite CsSnCl3 electrolyte. Figure 1 As shown, the XRD pattern matched the standard PDF card successfully, indicating successful doping and direct acquisition of cubic CsSnCl3. Figure 4 As shown, the antimony-doped CsSnCl3 electrolyte has an ionic conductivity of 3.58 × 10⁻⁶. -5 S cm -1 It has high room temperature ionic conductivity; such as Figure 5 As shown in d, the electronic conductivity is also relatively small, much smaller than the ionic conductivity.

[0052] A carbon current collector was prepared by mixing carbon nanotubes and graphene at a mass ratio of 9:1, and then pressed into a 12 mm radius disc in a glove box. A positive electrode was prepared by dropping vanadium oxychloride onto the current collector. Using the prepared polyviolet positive electrode as the working electrode, lithium metal as the counter electrode and reference electrode, and vanadium-doped tin halide perovskite CsSnCl3 solid prepared in this embodiment as the electrolyte, a blocking battery was assembled. Charge-discharge tests were performed using a Newway electrochemical workstation. Figure 8 As shown, the highest discharge specific capacity of the battery's positive electrode at a current density of 10 mA / g is 152 mAh / g.

[0053] Example 5

[0054] In an argon-filled glove box, cesium chloride, stannous chloride, and niobium chloride were mixed in a molar ratio of 1:0.5:0.5 and added to a 100ml stainless steel ball mill jar. The ball-to-material mass ratio was 40:1, and the milling speed was 350 rpm. Under sealed conditions, the mixture was transferred to a planetary ball mill for milling reaction for 1 hour, directly yielding niobium-doped cubic tin halide perovskite CsSnCl3 electrolyte. Figure 1 As shown, the XRD pattern matched the standard PDF card successfully, indicating successful doping and direct acquisition of cubic CsSnCl3. Figure 4 As shown, the niobium-doped CsSnCl3 electrolyte has an ionic conductivity of 1.68 × 10⁻⁶. -5 S cm -1 It has high room temperature ionic conductivity; such as Figure 5 As shown in Figure e, the electronic conductivity is also relatively small, much smaller than the ionic conductivity.

[0055] Example 6

[0056] In an argon-filled glove box, cesium chloride, stannous chloride, and neodymium chloride were mixed in a molar ratio of 1:0.6:0.4 and added to a 100ml stainless steel ball mill jar. The ball-to-material mass ratio was 20:1, and the milling speed was 400 rpm. Under sealed conditions, the mixture was transferred to a planetary ball mill for milling reaction, which lasted for 18 hours, directly yielding neodymium-doped cubic tin halide perovskite CsSnCl3 electrolyte. Figure 1 As shown, the XRD pattern matched the standard PDF card successfully, indicating successful doping and direct acquisition of cubic CsSnCl3. Figure 4 As shown, the neodymium-doped CsSnCl3 electrolyte has an ionic conductivity of 7.47 × 10⁻⁶. -5 S cm -1 It has high room temperature ionic conductivity; such as Figure 5 As shown in f, the electronic conductivity is also relatively small, much smaller than the ionic conductivity.

[0057] Example 7

[0058] In an argon-filled glove box, cesium chloride, stannous chloride, and ferric chloride were mixed in a molar ratio of 1:0.8:0.2 and added to a 100ml stainless steel ball mill jar. The ball-to-material mass ratio was 15:1, and the milling speed was 400 rpm. Under sealed conditions, the mixture was transferred to a planetary ball mill for milling reaction, which lasted for 12 hours, directly yielding an iron-doped cubic tin halide perovskite CsSnCl3 electrolyte. Figure 1 As shown, the XRD pattern matched the standard PDF card successfully, indicating successful doping and direct acquisition of cubic CsSnCl3. Figure 4 As shown, the iron-doped CsSnCl3 electrolyte has an ionic conductivity of 4.80 × 10⁻⁶. -5 S cm -1 It has high room temperature ionic conductivity; such as Figure 5 As shown in g, the electronic conductivity is also relatively small, much smaller than the ionic conductivity.

[0059] The active material, polyvioletin or a hydroxypiperidine compound, the conductive agent, acetylene black, and the binder, polyvinylidene fluoride, were thoroughly mixed in an appropriate amount of N-methylpyrrolidone solvent at a mass ratio of 8:1:1 to form a uniform slurry. This slurry was coated onto aluminum foil as a current collector and dried under vacuum at 80°C. The resulting material was then cut into 11mm diameter polyvioletin positive electrode sheets and hydroxypiperidine compound negative electrode sheets. Using the prepared polyvioletin positive electrode sheet as the working electrode and the hydroxypiperidine compound negative electrode sheet as the counter electrode and reference electrode, and the iron-doped tin halide perovskite CsSnCl3 solid prepared in this example as the electrolyte, a blocking battery was assembled. Charge-discharge tests were performed using a Newway electrochemical workstation. Figure 9 As shown, the highest discharge specific capacity of the battery's positive electrode at a current density of 10 mA / g is 76 mAh / g.

[0060] X-ray diffraction analysis

[0061] X-ray diffraction analysis was performed on the halotin-based perovskite CsSnCl3 electrolytes doped with one of the following elements: lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron, prepared in Comparative Examples and Examples 1-7. The results are as follows: Figure 1 As shown.

[0062] As can be seen from the figure, the undoped tin-halogen perovskite CsSnCl3 in the comparative example does not match the standard card, indicating that direct ball milling cannot obtain cubic phase CsSnCl3. However, the diffraction peaks of the tin-halogen perovskite CsSnCl3 electrolyte doped with one of the elements selected from lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron are consistent with the cubic crystal system tin-halogen perovskite CsSnCl3 standard card (PDF No. 22-0200), and no other impurity diffraction peaks are observed. This indicates that the prepared tin-halogen perovskite CsSnCl3 electrolyte doped with one of the elements selected from lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron is free of impurities, and the main phase is still tin-halogen perovskite CsSnCl3.

[0063] Ion conductivity test

[0064] The bismuth-doped tin halolithic perovskite CsSnCl3 electrolytes prepared in Comparative Examples and Examples 1-7 were installed in a blocked battery with stainless steel positive and negative electrodes. The solid electrolyte's bulk resistance Rb was measured using an electrochemical workstation. The ionic conductivity at different temperatures was calculated using a formula, and a graph of Logσ-1000 / T was plotted to obtain the relationship between ionic conductivity and temperature. It can be seen that the higher the temperature, the greater the ionic conductivity. Figure 4 Compared to the comparative example, the room-temperature ionic conductivity of halotin-based perovskite CsSnCl3 electrolytes doped with one of the following elements—lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron—was greater than 10. -5 S cm -1It has high ionic conductivity.

[0065] Based on the above tests, the inorganic solid electrolyte prepared by this invention for use in chloride-ion batteries has a wide electrochemical stability window, high ionic conductivity, and excellent chloride-ion conduction capability, demonstrating excellent intrinsic properties.

[0066] The rechargeable chloride-ion battery of the present invention has a high discharge specific capacity. It prevents the metal chloride from dissolving in the liquid electrolyte and causing the specific capacity to decay by using an inorganic solid electrolyte.

[0067] While the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the invention. Those skilled in the art can make various modifications and refinements without departing from the spirit and scope of the invention. Therefore, the scope of protection of the present invention shall be determined by the claims.

Claims

1. An inorganic solid electrolyte, characterized in that... The electrolyte is composed of element-doped tin-based perovskite CsSnCl3, wherein the doping element is one of lanthanum, antimony, bismuth, vanadium, niobium, neodymium, or iron.

2. The inorganic solid electrolyte according to claim 1, characterized in that... The molar percentage of the dopant element is 0.5% to 50%.

3. A method for preparing the inorganic solid electrolyte as described in claim 1, comprising the following specific steps: The chloride of the doped element was added to a ball mill jar and ball milled under an inert atmosphere for 0.5 to 24 hours to obtain an element-doped cubic tin halide perovskite CsSnCl3 inorganic solid electrolyte.

4. The method according to claim 3, characterized in that... The chlorine compounds used as dopants are lanthanum chloride, antimony chloride, bismuth chloride, vanadium chloride, niobium chloride, neodymium chloride, or ferric chloride.

5. The method according to claim 3, characterized in that... The ball-to-material mass ratio in the ball mill is 5–50:1, and the ball mill speed is 300–500 rpm.

6. The method according to claim 3, characterized in that... The inert atmosphere is nitrogen or argon.

Citation Information

Patent Citations

  • Method for preparing tin-based perovskite powder based on mechanochemical method

    CN113526545A

  • All-solid chloride ion battery and manufacturing method thereof

    JP2022126133A