A porous chitosan-based electrolyte for metal batteries and a preparation method thereof

By electrophoretically depositing chitosan nanosheets on a non-inert electrode to form a porous chitosan-based electrolyte, the problems of excessively large pore size and uneven ion migration in chitosan membranes are solved, resulting in an electrolyte matrix with high conductivity and excellent mechanical properties, suitable for metal batteries.

CN117638258BActive Publication Date: 2026-11-20EAST CHINA UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311620966.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-30
Publication Date
2026-11-20
Estimated Expiration
2043-11-30

AI Technical Summary

Technical Problem

Existing chitosan-based porous membranes generate excessively large bubbles during electrophoretic preparation, resulting in excessively large pore sizes. This makes it difficult to effectively suppress dendrite growth in metal batteries, and existing gel electrolytes cannot homogenize ion migration.

Method used

By replacing the inert electrode with a non-inert metal electrode, a porous membrane composed of chitosan nanosheets is prepared by electrophoretic deposition. Combined with electrolyte absorption, a porous chitosan-based electrolyte with interconnected pore structures is formed, which controls the pore size and porosity, inhibits dendrite growth, and homogenizes ion migration.

Benefits of technology

The process achieves nano-sizing and homogenization of chitosan membranes, improving electrical conductivity and mechanical properties, effectively suppressing dendrite growth, making it suitable as a gel electrolyte matrix for metal batteries, and facilitating large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117638258B_ABST
    Figure CN117638258B_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of new energy materials, and particularly relates to a porous chitosan-based electrolyte for metal batteries and a preparation method thereof. The porous chitosan-based electrolyte for metal batteries has a porous structure, excellent support performance, can homogenize ion mobility, and inhibit dendrite growth. The preparation method is to obtain a chitosan porous membrane by controllably depositing chitosan on a non-inert metal surface through electrophoresis technology, and then to prepare the porous chitosan-based electrolyte by absorbing an electrolyte. Compared with the existing chitosan electrophoresis technology, the method replaces the cathode inert electrode with a cathode non-inert electrode, promotes the uniform and rapid nucleation and precipitation of chitosan by limiting the generation of hydrogen bubbles and coupling transition metal complexation, and solves the defects of the existing chitosan porous membrane, such as large pore size and non-uniform pore structure. The metal battery using the porous chitosan-based electrolyte has an ideal cycle life, which is much better than the battery using a commercial separator.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of new energy materials technology, specifically relating to a porous chitosan-based electrolyte for metal batteries and its preparation method. Background Technology

[0002] In recent years, with the breakthroughs and rapid development of portable electronic devices such as mobile phones and laptops, the high performance and safety of energy storage devices have attracted increasing attention. As energy storage devices have developed, batteries have dominated the portable electronics market and changed our lives. However, today's energy storage devices are developing towards higher energy and higher safety, and ordinary batteries cannot meet our growing needs. Metal batteries have high theoretical capacity, low electrochemical potential and density, and are therefore considered the most promising energy storage technology, but their safety, cycle life, and other aspects still require further improvement.

[0003] Electrolytes are a crucial component of batteries, and their electrochemical and safety performance directly impacts battery usability. It is well known that liquid electrolytes are widely used in lithium-ion batteries, which currently dominate the market. When these liquid electrolytes are applied to metal batteries, the solvents and salts in the electrolyte readily react with the metal anode, forming an unstable solid-electrolyte interface on the anode surface. This solid-electrolyte interface is prone to defects, leading to dendrite growth and penetration of the separator, causing serious safety issues. Using gel electrolytes is considered an ideal solution to these problems because the free diffusion of solvents and salts in the gel is restricted by the network of polymer segments, while the abundant functional groups in the gel matrix promote the formation of a stable and dense solid-electrolyte interface on the metal electrode surface. Patents CN116231066 A and CN 116231056 A report self-healing gel electrolytes and gel electrolytes obtained through in-situ polymerization, respectively. Although these gel electrolytes possess the ability to repair dendrite penetration through the separator and avoid solvent contamination, they lack the ability to regulate ion migration, cannot homogenize the electrolyte ion flux on the metal electrode surface, and are unable to suppress dendrite growth.

[0004] Polymers with repeating monomers containing ionizable groups are called ionomers. As a matrix material for gel electrolytes, they can regulate the migration behavior of electrolyte ions through electrostatic interactions. Chitosan is a cationic polymer from biomass, possessing advantages such as environmental friendliness, natural origin, low cost, and biodegradability. Membrane materials made from chitosan have wide applications in energy, medicine, and bioscience. Because it can ionize into positive charges in solution, chitosan can be used to prepare membrane materials on the cathode side using electrophoretic deposition technology. For example, patents ZL201810082417.5 and ZL201710641263.4 propose methods for electrophoretically forming porous chitosan membranes on inert electrodes. However, due to the low hydrogen evolution overpotential on the inert electrodes used in existing methods, the gas production during electrophoresis is high, leading to excessively large bubbles within the membrane. The pore size of the prepared porous membrane exceeds 50 micrometers, which is extremely detrimental to its application as an electrolyte matrix in batteries. Therefore, based on some shortcomings of existing chitosan-based porous membranes and their electrophoretic preparation techniques, this invention proposes an ionic gel electrolyte with a controllable pore structure and its preparation method. Summary of the Invention

[0005] In order to overcome the shortcomings of the prior art, the main objective of this invention is to provide a porous chitosan-based electrolyte for metal batteries and a method for preparing the same.

[0006] The invention concept is as follows: A non-inert cathode electrode is used instead of an inert cathode electrode to suppress the generation of hydrogen bubbles. Simultaneously, due to the electrolysis side reaction, transition metal ions dissolved near the cathode can complex with chitosan molecules, thereby accelerating the nucleation and precipitation of chitosan. Through the combined effect of the aforementioned processes, the pore structure of the chitosan membrane is nanoscaled and homogenized, thus preparing a thin film suitable for a metal battery gel electrolyte substrate.

[0007] To achieve the above objectives, according to one aspect of the present invention, a porous chitosan-based electrolyte for metal batteries is provided, characterized in that the matrix of the porous chitosan-based electrolyte for metal batteries is composed of chitosan nanosheets stacked together, has a connected pore structure, a porosity of 60%~90%, and a conductivity of 15~45 mS·cm. -1 The porous chitosan-based electrolyte for metal batteries has a pore size of 20 nm to 4 μm and contains zinc ions, lithium ions, sodium ions, manganese ions, etc., in aqueous or organic solutions. The preparation method of the porous chitosan-based electrolyte for metal batteries is prepared by the following main steps: (1) Chitosan, hydrogen peroxide, and phosphate are dissolved in a protic acid aqueous solution to obtain an electrophoretic solution. (2) Constant voltage electrophoretic deposition is performed using a non-inert metal electrode as the cathode and an inert electrode as the anode to obtain a chitosan porous membrane on the surface of the non-inert metal electrode. (3) The prepared chitosan porous membrane is immersed in the electrolyte to fully absorb the electrolyte.

[0008] Furthermore, the metal battery includes a zinc metal battery, a lithium metal battery, and a sodium metal battery.

[0009] Furthermore, the electrolyte for the porous chitosan-based electrolyte used in the metal battery is one of the following: zinc chloride aqueous solution, lithium hexafluorophosphate solution, manganese sulfate aqueous solution, zinc sulfate aqueous solution, zinc trifluoromethanesulfonate aqueous solution, sodium hexafluorophosphate solution, and sodium perchlorate solution. The electrolyte absorption rate of the porous chitosan-based electrolyte used in the metal battery is 100%~300%.

[0010] Furthermore, in the electrophoretic solution of the method for preparing a porous chitosan-based electrolyte for metal batteries, the mass fraction of chitosan is 0.5%~2%, the mass fraction of added hydrogen peroxide is 0.3%~1.4%, the mass fraction of added phosphate is 0.1%~0.5%, and the protonic acid is one of hydrochloric acid, sulfuric acid, formic acid, and acetic acid, with a protonic acid concentration of 0.1M~0.5M.

[0011] Furthermore, the phosphate added to the electrophoretic solution in the method for preparing a porous chitosan-based electrolyte for metal batteries is one of sodium dihydrogen phosphate, disodium hydrogen phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate.

[0012] Furthermore, in the method for preparing a porous chitosan-based electrolyte for a metal battery, the non-inert metal electrode is one of an iron electrode, a zinc electrode, or a copper electrode, and the inert electrode is one of a stainless steel sheet, a platinum electrode, or a graphite electrode.

[0013] Furthermore, in the method for preparing a porous chitosan-based electrolyte for metal batteries, the electrophoresis voltage is 5V~60V and the electrophoresis time is 30s~600s.

[0014] Compared with conventional metal batteries, the porous chitosan-based electrolyte for metal batteries provided by this invention has the following advantages: (1) The electrolyte matrix obtained by chitosan electrophoresis has a porous structure and excellent support, and can absorb a large amount of electrolyte. The conductivity of the gel electrolyte is close to that of the liquid electrolyte. (2) The porous chitosan-based electrolyte has excellent mechanical properties and can resist dendrite penetration. Its uniform and dense pores can play a physical barrier role to inhibit dendrite growth. (3) Chitosan contains ionizable positively charged amino groups. Therefore, the electrolyte matrix formed by chitosan nanosheets has interconnected reasonable channels that can induce electrolyte ions in the pores to form an orderly flow field, thereby homogenizing ion mobility and inhibiting dendrite growth. (4) The electrophoresis technology used for porous chitosan-based electrolytes can easily control the porosity, pore size and thickness of the chitosan membrane. The electrophoresis technology is easy to scale up for production. Attached Figure Description

[0015] To more clearly illustrate the technical solutions of the present invention, the accompanying drawings used in the embodiments or comparative examples are briefly described below. The following drawings only include some embodiments and comparative examples involved in the description of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.

[0016] Figure 1 This is an electron microscope image of the porous chitosan-based electrolyte matrix prepared in Example 1 of the present invention.

[0017] Figure 2 This is an electron microscope image of the porous chitosan-based electrolyte matrix prepared in Comparative Example 1 of the present invention.

[0018] Figure 3 These are the charge-discharge curves obtained from the battery prepared in Example 1 and the battery prepared in Comparative Example 2 of this invention. Detailed Implementation

[0019] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0020] In the embodiments of the present invention, unless otherwise specified, the chemical reagents used can be obtained by purchasing or by preparing them using existing methods, and the instruments and equipment used are conventional equipment in the prior art.

[0021] Example 1

[0022] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and sodium dihydrogen phosphate were dissolved in a 0.12M acetic acid aqueous solution to obtain an electrophoresis solution. The mass fractions of chitosan, hydrogen peroxide, and sodium dihydrogen phosphate in the solution were 1%, 0.68%, and 0.3%, respectively. (2) Using a zinc electrode as the cathode and a stainless steel sheet as the anode, constant voltage electrophoretic deposition was performed at 30V for 120s to prepare a chitosan film on the zinc sheet, which is the porous chitosan-based electrolyte matrix. (3) The prepared porous chitosan membrane was immersed in a zinc sulfate aqueous solution to fully absorb the electrolyte.

[0023] The inventors further applied the chitosan electrolyte membrane prepared in this embodiment to a zinc metal battery. The positive electrode active material was manganese dioxide, and a zinc sheet was used as the negative electrode. The chitosan membrane was assembled as the electrolyte to obtain a zinc metal button battery. The assembled battery was left to stand for 24 hours, and its electrochemical performance was tested at a constant temperature of 25°C using a Newway battery testing system.

[0024] Figure 1The resulting porous chitosan-based electrolyte matrix is ​​composed of chitosan nanosheets, which have a connected pore structure, small pore size, and excellent mechanical properties.

[0025] Example 2

[0026] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and sodium dihydrogen phosphate were dissolved in a 0.12M acetic acid aqueous solution to obtain an electrophoresis solution. The mass fractions of chitosan, hydrogen peroxide, and sodium dihydrogen phosphate in the solution were 0.5%, 0.68%, and 0.2%, respectively. (2) Using a zinc electrode as the cathode and a stainless steel sheet as the anode, constant voltage electrophoretic deposition was performed at 30V for 120s to prepare a chitosan film on the zinc sheet, which is the porous chitosan-based electrolyte matrix. (3) The prepared porous chitosan membrane was immersed in a zinc sulfate aqueous solution to fully absorb the electrolyte.

[0027] Example 3

[0028] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and sodium dihydrogen phosphate were dissolved in a 0.12M acetic acid aqueous solution to obtain an electrophoresis solution. The mass fractions of chitosan, hydrogen peroxide, and sodium dihydrogen phosphate in the solution were 1%, 0.34%, and 0.2%, respectively. (2) Using a zinc electrode as the cathode and a stainless steel sheet as the anode, constant voltage electrophoretic deposition was performed at 30V for 120s to prepare a chitosan film on the zinc sheet, which is the porous chitosan-based electrolyte matrix. (3) The prepared porous chitosan membrane was immersed in a zinc sulfate aqueous solution to fully absorb the electrolyte.

[0029] Example 4

[0030] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and disodium hydrogen phosphate were dissolved in a 0.3M hydrochloric acid aqueous solution to obtain an electrophoresis solution. The mass fractions of chitosan, hydrogen peroxide, and disodium hydrogen phosphate in the solution were 0.5%, 0.2%, and 0.1%, respectively. (2) Using a zinc electrode as the cathode and a stainless steel sheet as the anode, constant voltage electrophoretic deposition was performed at 5V for 600s to prepare a chitosan porous membrane on the zinc sheet. (3) The prepared chitosan porous membrane was immersed in a zinc chloride aqueous solution to fully absorb the electrolyte.

[0031] Example 5 The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and ammonium dihydrogen phosphate were dissolved in a 0.5M acetic acid aqueous solution to obtain an electrophoretic solution. The mass fractions of chitosan, hydrogen peroxide, and ammonium dihydrogen phosphate in the solution were 2%, 1.5%, and 0.5%, respectively. (2) Using a copper electrode as the cathode and a graphite electrode as the anode, constant voltage electrophoretic deposition was performed at 60V for 30s to prepare a chitosan porous membrane on a copper sheet. (3) The prepared chitosan porous membrane was freeze-dried and then immersed in a lithium hexafluorophosphate solution to fully absorb the electrolyte.

[0032] Example 6

[0033] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and sodium dihydrogen phosphate were dissolved in a 0.12M acetic acid aqueous solution to obtain an electrophoresis solution. The mass fractions of chitosan, hydrogen peroxide, and sodium dihydrogen phosphate in the solution were 1%, 0.68%, and 0.1%, respectively. (2) Using a zinc electrode as the cathode and a stainless steel sheet as the anode, constant voltage electrophoretic deposition was performed at 30V for 120s to prepare a chitosan film on the zinc sheet, which is the porous chitosan-based electrolyte matrix. (3) The prepared porous chitosan membrane was immersed in a zinc sulfate aqueous solution to fully absorb the electrolyte.

[0034] Example 7

[0035] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and sodium dihydrogen phosphate were dissolved in a 0.12M acetic acid aqueous solution to obtain an electrophoresis solution. The mass fractions of chitosan, hydrogen peroxide, and sodium dihydrogen phosphate in the solution were 1%, 0.68%, and 0.15%, respectively. (2) Using a zinc electrode as the cathode and a stainless steel sheet as the anode, constant voltage electrophoretic deposition was performed at 30V for 120s to prepare a chitosan film on the zinc sheet, which is the porous chitosan-based electrolyte matrix. (3) The prepared porous chitosan membrane was immersed in a zinc sulfate aqueous solution to fully absorb the electrolyte.

[0036] Example 8

[0037] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and sodium dihydrogen phosphate were dissolved in a 0.12M acetic acid aqueous solution to obtain an electrophoresis solution. The mass fractions of chitosan, hydrogen peroxide, and sodium dihydrogen phosphate in the solution were 1%, 0.68%, and 0.2%, respectively. (2) Using a zinc electrode as the cathode and a stainless steel sheet as the anode, constant voltage electrophoretic deposition was performed at 30V for 120s to prepare a chitosan film on the zinc sheet, which is the porous chitosan-based electrolyte matrix. (3) The prepared porous chitosan membrane was immersed in a zinc sulfate aqueous solution to fully absorb the electrolyte.

[0038] Example 9

[0039] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and dipotassium hydrogen phosphate were dissolved in a 0.2M sulfuric acid aqueous solution to obtain an electrophoretic solution. The mass fractions of chitosan, hydrogen peroxide, and dipotassium hydrogen phosphate in the solution were 1.2%, 1.36%, and 0.4%, respectively. (2) Using a copper electrode as the cathode and a stainless steel sheet as the anode, constant voltage electrophoretic deposition was performed at 40V for 120s to prepare a chitosan porous membrane on the copper sheet. (3) The prepared chitosan porous membrane was freeze-dried and then immersed in a sodium hexafluorophosphate solution to fully absorb the electrolyte.

[0040] Example 10

[0041] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and ammonium dihydrogen phosphate were dissolved in a 0.25M formic acid aqueous solution to obtain an electrophoresis solution. The mass fractions of chitosan, hydrogen peroxide, and ammonium dihydrogen phosphate in the solution were 1.8%, 1.02%, and 0.2%, respectively. (2) Using an iron electrode as the cathode and a platinum electrode as the anode, constant voltage electrophoretic deposition was performed at 20V for 300s to prepare a chitosan porous membrane on an iron sheet. (3) The prepared chitosan porous membrane was freeze-dried and then immersed in a sodium perchlorate solution to fully absorb the electrolyte.

[0042] Example 11

[0043] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and sodium dihydrogen phosphate were dissolved in a 0.12M acetic acid aqueous solution to obtain an electrophoresis solution. The mass fractions of chitosan, hydrogen peroxide, and sodium dihydrogen phosphate in the solution were 1%, 0.68%, and 0.25%, respectively. (2) Using a zinc electrode as the cathode and a stainless steel sheet as the anode, constant voltage electrophoretic deposition was performed at 30V for 120s to prepare a chitosan film on the zinc sheet, which is the porous chitosan-based electrolyte matrix. (3) The prepared porous chitosan membrane was immersed in a zinc sulfate aqueous solution to fully absorb the electrolyte.

[0044] Example 12

[0045] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and sodium dihydrogen phosphate were dissolved in a 0.12M acetic acid aqueous solution to obtain an electrophoresis solution. The mass fractions of chitosan, hydrogen peroxide, and sodium dihydrogen phosphate in the solution were 1%, 0.68%, and 0.35%, respectively. (2) Using a zinc electrode as the cathode and a stainless steel sheet as the anode, constant voltage electrophoretic deposition was performed at 30V for 120s to prepare a chitosan film on the zinc sheet, which is the porous chitosan-based electrolyte matrix. (3) The prepared porous chitosan membrane was immersed in a zinc sulfate aqueous solution to fully absorb the electrolyte.

[0046] Example 13

[0047] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and sodium dihydrogen phosphate were dissolved in a 0.12M acetic acid aqueous solution to obtain an electrophoresis solution. The mass fractions of chitosan, hydrogen peroxide, and sodium dihydrogen phosphate in the solution were 1%, 0.68%, and 0.4%, respectively. (2) Using a zinc electrode as the cathode and a stainless steel sheet as the anode, constant voltage electrophoretic deposition was performed at 30V for 120s to prepare a chitosan film on the zinc sheet, which is the porous chitosan-based electrolyte matrix. (3) The prepared porous chitosan membrane was immersed in a zinc sulfate aqueous solution to fully absorb the electrolyte.

[0048] Example 14

[0049] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and diammonium hydrogen phosphate were dissolved in a 0.32M formic acid aqueous solution to obtain an electrophoretic solution. The mass fractions of chitosan, hydrogen peroxide, and diammonium hydrogen phosphate in the solution were 1%, 0.34%, and 0.3%, respectively. (2) Using an iron electrode as the cathode and a graphite electrode as the anode, constant voltage electrophoretic deposition was performed at 15V for 420s to prepare a chitosan porous membrane on an iron sheet. (3) The prepared chitosan porous membrane was immersed in a manganese sulfate aqueous solution to fully absorb the electrolyte.

[0050] Example 15

[0051] The specific steps of its preparation method are as follows: (1) Chitosan, hydrogen peroxide, and potassium dihydrogen phosphate were dissolved in a 0.1M sulfuric acid aqueous solution to obtain an electrophoretic solution. The mass fractions of chitosan, hydrogen peroxide, and potassium dihydrogen phosphate in the solution were 1.5%, 0.68%, and 0.4%, respectively. (2) Using a zinc electrode as the cathode and a graphite electrode as the anode, constant voltage electrophoretic deposition was performed at 45V for 90s to prepare a chitosan porous membrane on a zinc sheet. (3) The prepared chitosan porous membrane was immersed in a zinc trifluoromethanesulfonate aqueous solution to fully absorb the electrolyte.

[0052] Comparative Example 1

[0053] The preparation method is basically the same as that in Example 1, except that a platinum sheet is used as the cathode during constant voltage electrophoresis, and all other conditions are the same as in Example 1 to prepare a porous chitosan membrane and a porous chitosan-based electrolyte.

[0054] like Figure 2 As shown, the porous chitosan prepared in Comparative Example 1 has an extremely uneven pore structure, and the pore size is significantly larger than that in Example 1. It also has poor mechanical properties and cannot be used as an electrolyte matrix for metal batteries.

[0055] Comparative Example 2

[0056] The inventors used a glass fiber separator to replace the chitosan membrane in a zinc metal battery, with manganese dioxide as the positive electrode active material and zinc sheet as the negative electrode, to assemble a zinc metal button battery. The assembled battery was left to stand for 24 hours, and its electrochemical performance was tested at a constant temperature of 25°C using a Xinwei battery testing system.

[0057] The battery assembled in Example 1 at 0.5A g -1 After undergoing 2000 charge-discharge cycles at a current density of [value missing], its battery capacity retention was approximately 65%. In comparison, at 0.5 A g [value missing], [value missing] -1 At the specified current density, the battery was damaged after only about 250 cycles due to dendrite growth causing a short circuit. These results indicate that the electrolyte matrix obtained by chitosan electrophoresis on a non-inert electrode surface can suppress dendrite growth and prevent short circuits caused by dendrite growth.

[0058] Table 1

[0059]

[0060] As can be seen from Examples 1, 6, 7, 8, 11, 12, and 13 in Table 1, the higher the amount of sodium dihydrogen phosphate used, the larger the pore size of the electrolyte membrane. This is because the increased content of sodium dihydrogen phosphate enhances the electrostatic shielding effect between chitosan segments, resulting in larger channels in the chitosan membrane, leading to increased conductivity, decreased zinc ion transport number, and decreased tensile strength and elongation at break. Conversely, the higher the amount of hydrogen peroxide used, the greater the tensile strength of the electrolyte membrane and the lower the elongation at break.

[0061] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A porous chitosan-based electrolyte for metal batteries, characterized in that, The porous chitosan-based electrolyte for metal batteries has a matrix composed of chitosan nanosheets with interconnected pore structures, a porosity of 60% to 90%, a pore size of 100 nm to 4 μm, and an electrical conductivity of 15 to 45 mS·cm⁻¹. The electrolyte contained therein is an aqueous solution or organic solution containing zinc ions, lithium ions, sodium ions, or manganese ions.

2. The porous chitosan-based electrolyte for metal batteries according to claim 1, characterized in that, The metal batteries include zinc batteries, lithium batteries, and sodium batteries.

3. The porous chitosan-based electrolyte for metal batteries according to claim 1, characterized in that, The porous chitosan-based electrolyte for metal batteries contains one or more of the following electrolytes: zinc chloride aqueous solution, lithium hexafluorophosphate solution, manganese sulfate aqueous solution, zinc sulfate aqueous solution, zinc trifluoromethanesulfonate aqueous solution, sodium hexafluorophosphate solution, and sodium perchlorate solution; the electrolyte absorption rate of the porous chitosan-based electrolyte for metal batteries is 100% to 300% of the mass of the porous chitosan matrix.

4. The method for preparing a porous chitosan-based electrolyte for metal batteries according to claim 1, characterized in that, Its preparation process is as follows: (1) Dissolve chitosan, hydrogen peroxide, and phosphate in a protic acid aqueous solution to obtain an electrophoresis solution; (2) Using a non-inert metal electrode as the cathode and an inert electrode as the anode, constant voltage electrophoretic deposition was performed to obtain a chitosan porous membrane on the surface of the non-inert metal electrode. (3) Immerse the prepared chitosan porous membrane in the electrolyte to fully absorb the electrolyte until it reaches equilibrium swelling.

5. The preparation method according to claim 4, characterized in that, In step (1), the electrophoresis solution contains 0.5% to 2% chitosan, 0.2% to 1.5% hydrogen peroxide, 0.1% to 0.5% phosphate, and one of hydrochloric acid, sulfuric acid, formic acid, or acetic acid, with a concentration of 0.1 M to 0.5 M.

6. The preparation method according to claim 4, characterized in that, The phosphate added to the electrophoresis solution in step (1) is one of sodium dihydrogen phosphate, disodium hydrogen phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, ammonium dihydrogen phosphate, or diammonium hydrogen phosphate.

7. The preparation method according to claim 4, characterized in that, In step (2), the non-inert metal electrode is one of iron sheet, zinc sheet, and copper sheet, and the inert electrode is one of stainless steel sheet, platinum sheet, and graphite sheet.

8. The preparation method according to claim 4, characterized in that, In step (2), the electrophoresis voltage is 5V~60V and the electrophoresis time is 30s~600s.

Citation Information

Patent Citations

  • Chitosan chloride antibacterial material as well as preparation method and application thereof

    CN109316622A

  • Guided tissue regeneration membrane and its preparation method

    CN109395175B

  • Preparation method and application of high-voltage gel polymer electrolyte

    CN116231056A

  • Self-repairing gel polymer electrolyte and preparation method thereof

    CN116231066A

  • Core-shell structure carbon-silicon negative electrode material for lithium ion battery and preparation method of core-shell structure carbon-silicon negative electrode material

    CN114824201A