Method for making microstructured inserts for injection molding
By using low thermal conductivity resin materials and embossing technology to form inverted microstructures on the surface of lens mold inserts, the problems of weld lines and center distortion defects in injection molding are solved, achieving efficient and low-cost lens production.
Patent Information
- Application Number
- CN202280046643.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-07-13
- Filing Date
- 2022-07-12
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-07-12
AI Technical Summary
Existing injection molding methods are prone to weld lines and central distortion defects when preparing lenses with divergent geometries. In particular, the high thermal conductivity of the metal inserts causes the polymer melt to cool too quickly, making it difficult to achieve efficient and defect-free lens production.
Low thermal conductivity resin materials such as SU-8 are used to form microstructured mold inserts. Multiple inverted microstructures are formed on the surface of the mold inserts through embossing technology. Combined with appropriate processing steps and parameters, the occurrence of weld lines and center distortion defects is reduced during injection molding.
The use of low thermal conductivity mold inserts has been enabled, expanding the processing window, improving the flexibility and efficiency of lens production, reducing manufacturing costs, and effectively reducing weld lines and center distortion defects.
Smart Images

Figure CN117642264B_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to a method for manufacturing microstructured mold inserts for injection molding, particularly glass mold inserts having a microstructured resin film formed thereon. Background Technology
[0002] The "Background Art" description provided herein is intended to give a general overview of the background of this disclosure. To the extent that the work described in this Background Art section, and in aspects of this description that may not be considered prior art at the time of submission, the work of the currently nominated inventors is neither expressly nor implicitly acknowledged as prior art to this disclosure.
[0003] Injection molding of lenses with divergent geometries, such as -0.25 to -8.00 diopters, can present challenges that may introduce defects such as weld lines and central distortion defects. Figure 1 An exemplary cross-sectional schematic diagram of an exemplary prescription lens is shown. For example, Figure 1 The lens in this case could be a -6.0 diopter lens with a center thickness of 1.4 mm and an edge thickness of 10 mm. Injection molding of this lens geometry may result in a high level of internal stress due to differential shrinkage caused by the thicker edge compared to the thinner center.
[0004] Figure 2A A series of optical images showing the formation of weld line defects during lens manufacturing are presented. Figure 2B The central distortion defect is shown. Some mold inserts can be used to reduce the occurrence of such weld lines and central distortion defects by using materials with very low thermal conductivity. This prolongs the initial cooling rate to maintain the polymer melt temperature above the glass transition temperature (Tg) for a sufficient time and prolongs the solidification of the polymer melt. Conversely, metal inserts can immediately cool the polymer melt below Tg. This allows the molecular chains to relax to reduce internal stress, and the weld lines fuse together when the initial temperature is maintained above Tg.
[0005] Microstructured mold inserts fabricated by embossing can be inexpensive, precise, flexible, reproducible, and rapidly producible. When combined with mold insert materials having low thermal conductivity, this can lead to reduced quenching of the polymer during molding, as well as a reduction in weld lines and center distortion defects. Therefore, a method for forming microstructured mold inserts with low thermal conductivity and durability to withstand repeated injection molding cycles is desired, thereby extending service life without cracking, peeling, or delamination.
[0006] The aspects of this disclosure can be used in particular to address some of the aforementioned disadvantages in the art using the solutions set forth in the claims. Summary of the Invention
[0007] This disclosure relates to a method for forming a mold insert, the method comprising forming an impression having a surface including a plurality of inverted microstructures formed thereon; and pressing the impression into a membrane or medium disposed on the surface of a first mold insert to form a microstructured membrane, the microstructured membrane including a plurality of microstructures formed on the surface of the microstructured membrane based on the plurality of inverted microstructures, the plurality of microstructures being complementary to the plurality of inverted microstructures.
[0008] This disclosure also relates to a molding apparatus comprising a mold, the mold including a first mold insert and a second mold insert, the first mold insert including a microstructured film disposed on the surface of the first mold insert, the microstructured film including a plurality of microstructures formed thereon, wherein the material of the first mold insert is glass or metal, and the material of the microstructured film is resin, hybrid resin or mineral film, preferably SU-8.
[0009] It should be noted that this summary section does not detail every feature and / or progressively novel aspect of the disclosed or claimed invention. Rather, this summary section provides only a preliminary discussion of different embodiments and corresponding novel points. For additional details and / or possible perspectives on the embodiments, the reader may refer to the detailed description section of this disclosure and the corresponding drawings, which are discussed further below. Attached Figure Description
[0010] Various embodiments of the present disclosure, presented as examples, will be described in detail with reference to the following accompanying drawings, in which:
[0011] Figure 1 An exemplary cross-sectional schematic diagram of an exemplary prescription lens is shown.
[0012] Figure 2A A series of optical images showing the formation of weld line defects during lens manufacturing are presented.
[0013] Figure 2B The central distortion defect is shown.
[0014] Figure 3A An example of central distortion defect on a lens is shown.
[0015] Figure 3B An optical image of the fusion line defect condition is shown.
[0016] Figure 4 An exemplary schematic diagram of a mold insert comprising a plurality of microstructures formed thereon is shown within the scope of this disclosure.
[0017] Figure 5A An exemplary chemical structure of SU-8 within the scope of this disclosure is shown.
[0018] Figure 5B An exemplary chemical structure of γ-butyrolactone (GBL) within the scope of this disclosure is shown.
[0019] Figure 5C An exemplary chemical structure of bis[4-(diphenylsulfonium)phenyl]sulfide bis(hexafluoroantimonate) is shown within the scope of this disclosure.
[0020] Figure 5D An exemplary chemical structure of 4-phenylthiophenyl diphenylsulfonium hexafluoroantimonate is shown within the scope of this disclosure.
[0021] Figure 5E An exemplary schematic diagram of a cured network of SU-8 including GBL is shown within the scope of this disclosure.
[0022] Figure 6A An exemplary cross-sectional schematic diagram of an exemplary mold-making method within the scope of this disclosure is shown.
[0023] Figure 6B An exemplary cross-sectional schematic diagram of an exemplary impression-making method by injection molding is shown within the scope of this disclosure.
[0024] Figure 6C An exemplary cross-sectional schematic diagram of an exemplary mold-making method by machining and deposition within the scope of this disclosure is shown.
[0025] Figure 7 An exemplary cross-sectional schematic diagram of an exemplary resin film formation method within the scope of this disclosure is shown.
[0026] Figure 8 An exemplary cross-sectional schematic diagram of an exemplary resin film imprinting method within the scope of this disclosure is shown.
[0027] Figure 9 An exemplary graph of the pressure and temperature distribution within the scope of this disclosure is shown.
[0028] Figure 10 An exemplary cross-sectional schematic diagram of an exemplary impression removal process within the scope of this disclosure is shown.
[0029] Figure 11 An exemplary cross-sectional schematic diagram of an exemplary mold insert undergoing UV curing within the scope of this disclosure is shown.
[0030] Figure 12 An exemplary cross-sectional schematic diagram of an exemplary mold insert that has undergone post-exposure baking (PEB) within the scope of this disclosure is shown.
[0031] Figure 13AAn exemplary cross-sectional schematic diagram of an exemplary injection molding method using a first mold insert having a microstructured resin film within the scope of this disclosure is shown.
[0032] Figure 13B Exemplary cross-sectional profiles of two microstructures within the scope of this disclosure are shown.
[0033] Figure 14 Differential scanning calorimetry (DSC) plots for various examples are shown.
[0034] Figure 15 Microscopic images and microstructure outlines of inverted microstructures obtained on PDMS impressions used in Examples 6 to 12 are shown.
[0035] Figure 16 An optical image of the replicated microstructure from the SU-8 layer of Example 9 is shown.
[0036] Figure 17 Microscopic images and microstructure outlines of inverted microstructures obtained on PDMS impressions used in Examples 13 and 14 are shown.
[0037] Figure 18A Microstructure optics results for measuring the optical power of each microstructure for lenses in Examples 15 and 16 are shown.
[0038] Figure 18B Microscopic images and microstructure profiles of the lens produced by Example 12 are shown.
[0039] Figure 19 It is an optical image of the master mold, including its microstructure.
[0040] Figure 20 This is a schematic diagram of the master mold including PDMS filled in the gasket.
[0041] Figure 21 It is an optical image of the master mold including PDMS filled in the gasket.
[0042] Figure 22A It is an optical image of the first mold insert of the part of the machining process.
[0043] Figure 22B It is the first mold insert with a finely machined surface.
[0044] Figure 23 It is an optical image of the mold holding device.
[0045] Figure 24 It is an optical image of the impression pressed into the resin film during the curing process.
[0046] Figure 25It is an optical image of the first mold insert, which includes a microstructured resin film.
[0047] Figure 26 It is an optical image of the first mold insert with a partially delaminated microstructured resin film.
[0048] Figure 27A It is an optical image of a copper layer with a thickness of 40 nm deposited on a glass mold insert.
[0049] Figure 27B It is an optical image of an MR8 substrate including an embossed hard coating.
[0050] Figure 27C It is an optical image of the imprinted phenolic film.
[0051] Figure 28 This is an exemplary flowchart of a method for fabricating microstructured inserts within the scope of this disclosure. Detailed Implementation
[0052] The following disclosure provides numerous different variations or examples for implementing various features of the proposed subject matter. Specific examples of components and arrangements are described below to simplify this disclosure. These components and arrangements are merely examples and are not intended to be limiting, nor are they contingent on being operable together in any arrangement. Unless otherwise indicated, the features and embodiments described herein can be operated together in any arrangement. For example, forming a first feature on or over a second feature in the following description may include embodiments where the first and second features are formed in direct contact, and may also include embodiments where an additional feature may be formed between the first and second features such that the first and second features are not in direct contact. Additionally, reference numerals and / or letters may be repeated in various examples in this disclosure. Such repetition is for simplicity and clarity and does not in itself define the relationship between the various embodiments and / or configurations discussed. Furthermore, for ease of description, spatial relative terms such as “top,” “bottom,” “below,” “under,” “lower,” “above,” “upper,” etc., may be used herein to describe the relationship between one element or feature and another element(s)(s) shown in the figures. These spatial relative terms are intended to cover different orientations of the device in use or operation, in addition to the orientations depicted in the figures. The device of the present invention can be oriented in other ways (rotated 90 degrees or otherwise) and the spatial relative descriptive terms used herein can also be interpreted accordingly.
[0053] For clarity, the order of discussion of the different steps described herein has been presented. Generally, these steps can occur in any suitable order. Furthermore, although each of the different features, techniques, configurations, etc., herein may be discussed in different places within this disclosure, it is intended that each concept can be implemented independently of or in combination with each other. Accordingly, the invention can be practiced and observed in many different ways.
[0054] As previously mentioned, weld lines and center distortion defects can occur during the lens molding process due to increased cooling of the injected polymer melt. Typically, weld lines can form during injection when the leading edge of the polymer melt encounters another leading edge, potentially originating from multiple gates filling the mold cavity. Therefore, this can lead to head-on collisions of individual flow fronts of the polymer melt, or splitting and convergence of the flow front due to the presence of obstructions or excessive lateral part thickness variations.
[0055] As previously described, during the injection molding of prescription lenses, weld lines and center distortion defects can occur due to the rapid cooling of the injected polymer melt and the presence of multiple flow fronts. For example, Figure 3A An example of central distortion defect on a -6.0D lens produced using a metal insert is shown, and Figure 3B An optical image of a weld line defect condition obtained on a -6.0D lens using a metal insert is shown.
[0056] Metal inserts used for injection molding, such as nickel-phosphorus (NiP) plated steel inserts, may include surfaces with microstructures machined by diamond turning. Figure 4An exemplary schematic diagram of a mold insert comprising a plurality of microstructures 695 formed thereon, available within the scope of this disclosure, is shown. The plurality of microstructures 695 may be refractive, diffractive, or discontinuous on a portion or the entire surface of the insert. In one example, the mold insert may be copper, and the plurality of microstructures 695 are formed using alternative methods such as diamond turning (e.g., etching). In another example, the mold insert may be fused silica or photosensitive resin, and the plurality of microstructures 695 are formed by photolithography. Notably, depending on the material, imprinting can also enable a wide variety of designs on the surface of the mold insert. Metal inserts can provide successful replication of optical microstructures on lenses for myopia control applications. However, due to the higher thermal conductivity of metal inserts, specific processing conditions with tighter tolerances may be required to successfully transfer the pattern of the metal insert to the resulting lens while maintaining a defect-free state. Therefore, injection molding lenses with different geometries within a multi-cavity mold can be challenging because each geometry can include different fabrication schemes with different optimal parameters, and only a tight set of process parameters can be used with a specific metal insert within the multi-cavity mold. Conversely, mold inserts with lower thermal conductivity can provide an expanded processing window to allow for the fabrication of a wider range of lenses. This can provide increased flexibility during fabrication to increase efficiency and productivity, as well as ease of implementation in more products. Furthermore, using resins as described herein to produce microstructured insert replicas can reduce the cost of fabricating additional replicas of mold inserts made by machining NiP-plated steel.
[0057] Within the available resources, UV-sensitive resins or resins including epoxy functional groups can be used to form the mold insert. For example, the resin can be SU-8. The mold insert can be formed from a master mold, such as the previously described NiP-plated steel insert with multiple microstructures 695 formed thereon. It is understood that various types of master molds can be used, such as other mold inserts used during injection molding.
[0058] As described herein, resins, hybrid resins, or mineral oil films can be used to form low thermal conductivity microstructured mold insert surface films replicated from microstructured NiP steel master molds used for injection molding. For example, SU-8 resin is used. A method including various processing steps and parameters is described to facilitate the accurate replication of multiple microstructures 695 on the master mold. A chemical description is also described herein.
[0059] Figure 5A An exemplary chemical structure of SU-8, available within the scope of this disclosure, is shown. SU-8 is an epoxy resin having an octafunctional epoxy molecule and is sensitive to UV light and heat in the presence of a suitably selected cationic initiator.
[0060] Figure 5BAn exemplary chemical structure of γ-butyrolactone (GBL), which is available within the scope of this disclosure, is shown. GBL is a reactive diluent for mixing with SU-8 resin.
[0061] Figure 5C An exemplary chemical structure of bis[4-(diphenylsulfonium)phenyl]sulfide bis(hexafluoroantimonate) is shown, which is available within the scope of this disclosure. Bis[4-(diphenylsulfonium)phenyl]sulfide bis(hexafluoroantimonate) is a photoinitiator mixed with SU-8 resin.
[0062] Figure 5D An exemplary chemical structure of 4-phenylthiophenyl diphenylsulfonium hexafluoroantimonate, which is available within the scope of this disclosure, is shown. 4-phenylthiophenyl diphenylsulfonium hexafluoroantimonate is also a photoinitiator for mixing with SU-8 resin.
[0063] In the above, GBL is a reactive diluent that undergoes ring-opening and reaction with epoxy groups during exposure to UV light. The amount of GBL in the final cured film affects the film's glass transition temperature (Tg) and storage modulus. GBL can act as a bridge within the SU-8 molecule, from one epoxy group to another or from one molecule of SU-8 to another. The final Tg can be increased with lower GBL amounts, but it can also become less robust and more difficult to cure completely. Therefore, the description aims to depict the optimal concentration of GBL and the corresponding processing steps to provide suitable microstructured inserts for injection molding.
[0064] Figure 5E An exemplary schematic diagram of a cured SU-8 network comprising GBL, available within the scope of this disclosure, is shown. For example, the SU-8 network may comprise 0% to 50% GBL, or 0% to 40% GBL, or 0% to 30% GBL, or 0% to 20% GBL, or 0% to 10% GBL, or 0% GBL, or 33% GBL (as shown). Within the available range, introducing more GBL can reduce the number of available epoxy groups, while introducing less GBL increases the difficulty of epoxy group reaction due to reduced polymer network mobility. For the latter, a higher post-baking temperature can be used to ensure complete reaction of the epoxy (SU-8) groups, and this, in turn, will result in a higher Tg for the mold insert.
[0065] Within the available range, mold inserts with microstructured films formed from SU-8 can have a thickness of 0.2 Wm. -1 K -1 Thermal conductivity, thermal expansion less than 100 ppm / K, Tg from 100 °C to undetectable based on GBL concentration and post-baking, and elastic modulus (Young's modulus) of 4 to 5 GPa based on GBL concentration and post-baking.
[0066] Within acceptable limits, the coefficient of thermal expansion of the SU-8 film can be similar to that of the mold insert material, which would otherwise be susceptible to delamination due to thermal shock during injection molding. Excessive shrinkage of the SU-8 can also lead to delamination during post-baking. For this reason, the insert base material, SU-8 film thickness, the silica nanoparticle content in the SU-8, and the processing steps for preparing the cured SU-8 (i.e., GBL content and post-baking conditions) can be optimized for final injection molding. The fabrication method of the microstructured SU-8 film will now be explained.
[0067] Figure 6A An exemplary cross-sectional schematic diagram of an exemplary mold-making method available within the scope of this disclosure is shown. Within the scope of availability, reference is made to... Figure 6A The first step may involve applying a gasket 605, such as tape, around the master mold 610 to form a well 620. For example, the master mold 610 is a NiP-plated steel insert and includes multiple microstructures 695. As previously described, the multiple microstructures 695 may be refractive, diffractive, or discontinuous on a portion or the entire surface of the insert. In one example, the master mold 610 may be copper, and the multiple microstructures 695 are formed using alternative methods such as diamond turning (e.g., etching). In another example, the master mold 610 may be fused silica or photosensitive resin, and the multiple microstructures 695 are formed by photolithography. Figure 6A In the second step, trap 620 can be filled with a thermosetting resin. For example, the resin can be polydimethylsiloxane (PDMS). Figure 6A In the third step, the master mold and the thermosetting resin filled in the trap 620 can be cured in an oven to form an impression 615. The thermosetting resin can replicate multiple inverted microstructures 695 on the surface of the master mold 610. Figure 6A In the fourth step, the washer 605 can be removed and the impression 615 can be detached from the master mold. The impression 615 replicates the surface of the master mold 610 to form multiple inverted microstructures 690.
[0068] Microstructures may include microlenses, miniature lenses, bifocal lenses, or progressive lenses, or any other type of structure or element having a physical Z-shape / height between 0.1 μm and 50 μm and a width / length between 0.5 μm and 3.0 mm. These structures preferably have a periodic or pseudo-periodic layout, but may also have random positions. Preferred layouts of the microstructures may be grids with constant grid step sizes, honeycomb layouts, multiple concentric rings, or continuous structures, for example, without space between microstructures. These structures can provide wavefront modification in terms of intensity, curvature, or optical deviation, wherein the wavefront intensity is configured such that the structure can be absorbent and can locally absorb wavefront intensity in the range of 0% to 100%, wherein the curvature is configured such that the structure can locally modify the wavefront curvature in the range of + / -20, 500, or 1000 diopters, and the optical deviation is configured such that the structure can locally scatter light at angles from + / -1° to + / -30°. The distance between structures can range from 0 (continuous) to 3 times the size of the structure in the X and / or Y dimensions (separate microstructures).
[0069] In the sense of this disclosure, two optical elements are considered continuous if there exists a path supporting and connecting two optical elements located on the surface of the lens substrate, and if the path does not reach the base surface where the optical elements are located. According to another scope, an optical element on the pupil is continuous when it does not include a refractive region having a refractive power based on a prescription for the wearer's eye, or includes a refractive region consisting of multiple correspondingly independent island-like regions having a refractive power based on a prescription for the wearer's eye. According to another scope, two optical elements are considered continuous if there exists a path connecting them, and a portion of the path cannot be used to measure refractive power based on a prescription for the human eye. According to another scope, the continuity of an optical element can also be defined in terms of its surface. Consideration is given to a measured surface of 3 mm. 2 Up to 10mm 2 Between. The measurement surface includes X optical elements / mm. 2 The density. If at least 95%, preferably 98%, of the tested surface has a different optical power than the surface where the optical element is located, then the optical element is considered to be continuous.
[0070] Furthermore, the microstructures forming the microstructured main surface of the ophthalmic lens substrate can include lenticules. Lenticules can form protrusions and / or depressions (which can be either protruding or recessed structures) on the main surface to which they are disposed. The profile of the lenticules can be circular or polygonal, such as hexagonal. More specifically, lenticules can be microlenses. Microlenses can be spherical, toric, or have an aspherical shape. Microlenses can have a single focal point, or cylindrical power, or a non-focal point. Microlenses can be used to prevent the progression of myopia or hyperopia. In this case, the base lens substrate includes a base lens providing optical power for correcting myopia or hyperopia, and respectively, if the wearer is myopic, the microlens can provide optical power greater than that of the base lens, or if the wearer is hyperopic, the microlens can provide optical power less than that of the base lens. Lenticules can also be Fresnel structures, diffractive structures (such as microlenses defining each Fresnel structure), permanent technical protrusions (protruding structures), or phase-shifting elements. Microlenses can also be refractive optical elements such as microprisms and light-diffusing optical elements such as small protrusions or cavities, or any type of element that creates roughness on a substrate. It can also be a π-Fresnel microlens as described in US 2021109379, i.e., a Fresnel microlens with a π phase jump in its phase function at the nominal wavelength, as opposed to a single-focus Fresnel lens with multiple values of 2π for the phase jump. Such microlenses include structures with discontinuous shapes. In other words, the shape of such a structure can be described by a height function, exhibiting discontinuities in distance from the reference plane of the principal surface of the optical lens to which the microlens belongs, or by a derivative exhibiting discontinuities. Within the scope of availability, microstructures can be branding marks, holographic marks, metasurfaces, etc.
[0071] Microlenses can have an external shape that can be inscribed within a circle with a diameter greater than or equal to 0.5 micrometers (μm) and less than or equal to 1.5 millimeters (mm). Microlenses have a height, measured in a direction perpendicular to their main surface on which they are arranged, greater than or equal to 0.1 μm and less than or equal to 50 μm. Microlenses can have a periodic or pseudo-periodic layout, but can also have random positions. One layout of microlenses can be a grid with a constant grid step size, a honeycomb layout, multiple concentric rings, or continuous, for example, without space between microstructures. These structures can provide wavefront modification in terms of intensity, curvature, or optical deviation, wherein the wavefront intensity is configured such that the structure can be absorptive and can locally absorb wavefront intensity in the range of 0% to 100%, wherein the curvature is configured such that the structure can locally modify the wavefront curvature in the range of + / -20, 500, or 1000 diopters, and the optical deviation is configured such that the structure can locally scatter light at angles from + / -1° to + / -30°. The distance between structures can range from 0 (continuous) to 3 times the distance between structures (separate microstructures).
[0072] Figure 6B An exemplary cross-sectional schematic diagram of an exemplary impression-making method by injection molding, available within the scope of this disclosure, is shown. Within the available scope, a master mold 610 is used as one side of a mold having a first mold side 625 and a second mold side 630. The mold may include a first mold insert 635 disposed on the first mold side 625 and a second mold insert 640 disposed on the second mold side 630. Figure 6B In the first step, the master mold 610 may replace the first mold insert 635 and is configured to engage with the second mold insert 640. In one example, the master mold 610 replacing the first mold insert 635 may be formed by die casting or CNC machining or any other method known in the art, and subsequently diamond turning to produce a metasurface, multiple microstructures 695. In other examples, the multiple microstructures 695 on the master mold 610 may be formed based on the material of the master mold 610 by processes such as etching, photolithography, additive manufacturing, and embossing. The second mold insert 640 may be made by methods known in the art such as CNC machining, die casting, etc., to form a complementary part of the mold for injection molding. Figure 6B In the second step, the female mold 610 and the second mold insert 640 can be joined to form a cavity, and thermosetting resin can be injected into the cavity to form an impression 615. Figure 6B In the third step, the thermosetting resin can be cooled, and then the mold 615 can be disengaged when the female mold 610 and the second mold insert 640 are disconnected.
[0073] Figure 6CAn exemplary cross-sectional schematic diagram of an exemplary impression-making method by machining and deposition, available within the scope of this disclosure, is shown. Within the available scope, the impression 615 can be formed by metal machining and vacuum deposition. Figure 6C In the first step, the metal blank is machined to the desired basic curvature. Figure 6C In the second step, the metal blank can be plated with, for example, NiP. Figure 6C In the third step, multiple inverted microstructures 690 can be machined into the NiP coating. Figure 6C In the fourth step, a low surface energy nanolayer film can be deposited on the NiP coating. For example, vacuum deposition processes such as physical vapor deposition (PVD), chemical vapor deposition (CVD), electron beam evaporation, atomic layer deposition, sputtering, and plasma-enhanced PVD can be performed. It is understood that the mold 615 can also be formed by machining or photolithography. The mold can be a film with uniform or non-uniform thickness.
[0074] Within the scope of availability, the material of impression 615 may include any material that is sufficiently rigid yet does not strongly adhere to SU-8 or master mold 610, and precisely replicates the multiple microstructures 695 on master mold 610. Examples of low surface energy impression 615 materials produced by casting or coating include PDMS, fluorinated ethylene propylene (FEP), and polytetrafluoroethylene (PTFE). Examples of impression 615 materials produced by injection molding include polymethyl methacrylate (PMMA), cyclic olefin copolymers (COC), polymethylpentene (PMP), and polystyrene. Notably, layered forms may include combinations of multiple layers of the above materials. For example, a 2-layer impression 615 may include PMMA and PMP. The material of impression 615 may have an elastic modulus greater than 0.5 MPa. Within the scope of availability, the difference between the base arc of impression 615 and the base arc of the first mold insert 635 is within ±0.5 diopters. That is, the base arc of the impression 615 can be slightly higher or lower than the base arc of the mold insert 635 to optimize replication, quality, etc. Other materials for the impression 615 may include glass, steel, aluminum, or metal alloys.
[0075] It is worth noting that Figure 6C This is an example of a NiP-plated metal insert having a convex surface comprising multiple inverted microstructures 690 (instead of multiple microstructures 695). This is an example of directly fabricating the metal insert as a mold 615 to eliminate the need for casting / coating or injection molding to manufacture the mold 615. Therefore, the structure is inverted. Resin, such as SU-8, may adhere to the NiP. Therefore, the NiP plating can be treated to reduce the surface energy so that SU-8 does not adhere. Thus, a functional film with low surface energy can be applied by vacuum deposition. For example, the mold 615 (for...) Figures 6A-6C The surface energy can be less than 50 dynes / cm, or less than 40 dynes / cm, or 0 to 30 dynes / cm.
[0076] As the impression 615 is formed, the surface of the first mold insert 635 can be modified to receive the embossing of multiple inverted microstructures 690. For this purpose, Figure 7 An exemplary cross-sectional schematic diagram of an exemplary resin film formation method available within the scope of this disclosure is shown. Figure 7 In the first step, a first mold insert 635 is arranged in a spin coater configured to rotate the first mold insert 635 about a rotation axis at a predetermined rotational speed. For example, the predetermined rotational speed can be in the range of 500 RPM to 10,000 RPM. The spin coater can ramp up and down the predetermined rotational speed over a certain period of time and can also maintain the predetermined rotational speed for a certain period of time. That is, a predefined rotation curve can be used based on the desired coverage and thickness of the resulting resin film or medium 645. Figure 7 In the second step, resin can be deposited on the surface of the first mold insert 635, and the first mold insert 635 can be rotated at a predetermined rotational speed or a predefined rotational curve to form a resin film or medium 645. Figure 7 In the third step, the resin film or medium 645 can be soft-baked in an oven to remove the solvent from the resin film or medium 645.
[0077] As previously mentioned, the rotation speed and, additionally, the GBL content can determine the thickness of the resin film or medium 645. For example, with a GBL content close to 40%, the thickness can be 20 μm at 1500 RPM or 10 μm at 3000 RPM. Lower thicknesses can be obtained at higher GBL contents. Soft baking in an oven can promote the removal / evaporation of GBL from the resin film or medium 645. It is understood that the above steps can be repeated to gradually build up the final layer thickness of the resin film or medium 645. Applying the medium 645 by, for example, doctor blade, inkjet printing, dip casting, spraying, spin coating, film coating, or lamination can produce thicknesses between 0.1 μm and 300 μm.
[0078] In addition, other processes can be performed to improve coating quality and adhesion to the desired surface. For example, plasma treatment of the first mold insert 635 and / or incorporation of solvents into the resin formulation can improve wettability to control pinhole coating problems.
[0079] Figure 8An exemplary cross-sectional schematic diagram of an exemplary resin film or medium 645 imprinting method available within the scope of this disclosure is shown. Heat can be applied to soften the uncured resin film or medium 645 to improve the replication accuracy of the impression 615. For example, heat can be applied between 10°C and 250°C, or 15°C and 200°C, or 50°C and 180°C to improve the replication quality of the plurality of microstructures 695 (i.e., the impression 615 comprising a plurality of inverted microstructures 690 is imprinted onto the resin film or medium 645 to transfer a pattern of the plurality of microstructures 695). Replication can be optimized with an appropriate distribution of pressure and temperature relative to time. For example, pressures between 1 and 8000 psi, or greater than 8000 psi, can be used depending on the temperature used and the size of the microstructures. The elastic modulus (or stiffness) of the impression 615 material can be high enough to not deform under these applied pressures during stamping, otherwise, if the impression 615 deforms, the plurality of microstructures 695 may not be replicated well. For example, for impression 615 material exposed to these pressures, an elastic modulus between 2 MPa and 200 GPA may be required.
[0080] Furthermore, alignment is important for maintaining the pattern and concentric arrangement of the multiple microstructures 695 with the optical center of the first mold insert 635. For this purpose, the mold 615 can be placed on the first fixture 650, and the first mold insert 635 coated with a resin film or medium 645 can be placed on the second fixture 655. It should be noted that the medium 645 can be pressed using a mold such as the mold 615 to obtain a coating or film configuration. Both the mold 615 on the first fixture 650 and the first mold insert 635 on the second fixture 655 can be placed in an oven during the imprinting process, such as... Figure 8 As shown in the diagram. The first fixing device 650 and the second fixing device 655 may include features configured to engage while maintaining alignment of the first fixing device 650 and the second fixing device 655. For example, the first fixing device 650 may include an alignment hole, and the second fixing device 655 may include an alignment post, wherein inserting the alignment post into the alignment hole facilitates alignment of the centers of the first fixing device 650 and the second fixing device 655 during engagement of the first fixing device 650 and the second fixing device 655 (and the attached corresponding impression 615 and the first mold insert 635). It is understood that if the operator is able to maintain the center alignment of the impression 615 and the first mold insert 635 during imprinting, the first fixing device 650 and the second fixing device 655 are not required. Figure 8 As shown, the mold 615 can be pressed into a resin film or medium 645 to form a first mold insert 635 with a microstructured surface.
[0081] Figure 9An exemplary diagram of exemplary pressure and temperature distributions available within the scope of this disclosure is shown. The pressure of the impression 615 pressed into the resin layer can be maintained by any mechanism. For example, pressure can be applied to the impression 615 using a pneumatic or hydraulic piston or a flexible bladder. The flexible bladder can promote uniform pressure such that the force vector is perpendicular to the base arc of the first mold insert 635 in all areas of the impression 615. Furthermore, the temperature and pressure distribution can be optimized to provide optimal replication. For example, Figure 9 It shows a dynamic rather than static distribution, where pressure and temperature vary throughout the cycle.
[0082] Furthermore, the entire stamping process can be automated through machine control and design to achieve precise timing of heat and pressure. For example, the resin film or medium 645 and the mold 615 can be preheated after being soft-baked under an infrared (IR) type heater. The IR heater can then be removed immediately, either mechanically or automatically, followed by the stamping step. This allows for faster cooling of the stamped resin film or medium 645 and promotes a more precise distribution of temperature and pressure over time.
[0083] Figure 10 An exemplary cross-sectional schematic diagram of an exemplary impression release process available within the scope of this disclosure is shown. At room temperature, the uncured resin film or medium 645 can be in a glassy state, and the impression 615 can be removed. For example, the adhesion of the PDMS impression 615 to the SU-8 resin film or medium 645 can increase after UV exposure. Therefore, it is preferable to remove the PDMS impression 615 before curing the SU-8 resin film or medium 645. Typically, the impression 615 can have a low surface energy for detachment from the surface of the resin film or medium 645. Alternatively, the impression 615 can be made of metal and then vacuum-coated with a thicker release nanolayer. This can provide an impression 615 with both a very high modulus suitable for extreme stamping pressure ranges and very good release properties for detachment from the SU-8 resin film or medium 645. An advantage of embossing is the ability to bring a wide variety of designs to the surface of the mold insert.
[0084] Furthermore, the ability of the mold 615 to be removed before UV exposure means that the mold 615 does not require high transparency to UV. However, if it is desired that the mold 615 can be removed after UV exposure, then the mold 615 must have high transparency to UV exposure.
[0085] Within the scope of availability, a resin film or medium 645 can be formed on an auxiliary component (such as a glass mold part), and an impression 615 can be pressed into the resin film or medium 645 on the auxiliary component. Furthermore, the auxiliary component can be inserted adjacent to the first mold insert during injection molding to provide a removable and interchangeable microstructured auxiliary component. In addition, the auxiliary component can provide flexibility and ease of use during manufacturing processes, such as during spin coating or baking. Compared to the first mold insert 635, the auxiliary component also offers the advantage of easy replacement.
[0086] Figure 11 An exemplary cross-sectional schematic diagram of an exemplary mold insert available within the scope of this disclosure undergoing UV curing is shown. Within the scope of availability, a first mold insert 635 having a microstructured resin film or medium 645 can be UV cured. As previously mentioned, a high UV transparency material for the impression 615 can be used to allow the impression 615 to remain pressed into the resin film or medium 645 during UV curing. A material with a UV transparency of 0.2 to 10 J / cm² can be used during development. 2 The exposure energy is near UV (e.g., 350-400 nm). Alternatively, a pulsed UV system can be used to avoid overheating and distortion of the microstructured resin film or dielectric 645. Curing and post-baking the dielectric 645 can produce thicknesses between 0.1 μm and 300 μm.
[0087] Figure 12 An exemplary cross-sectional schematic diagram of an exemplary mold insert available within the scope of this disclosure undergoing exposure-after baking (PEB). Within the available scope, a first mold insert 635 having a microstructured resin film or medium 645 can be baked to fully crosslink the epoxy groups in the resin film or medium 645. This can help solidify multiple microstructures 695, which can again help give them refractive or diffractive properties. Similarly, the pattern can be discontinuous on a portion or the entire surface of the first mold insert 635. During UV exposure, only some epoxy groups are crosslinked because the network becomes too rigid, thus preventing unreacted epoxy groups from contacting. With sufficient PEB, the increased conversion rate of epoxy crosslinking improves properties such as Tg. However, if the PEB temperature is too high, the epoxy crosslinking conversion rate will be too high, leading to excessive shrinkage, stress accumulation and potential deformation of the microstructures, or delamination of the microstructured resin film or medium 645 from the first mold insert 635.
[0088] Figure 13AAn exemplary cross-sectional schematic diagram of an exemplary injection molding method using a first mold insert 635 having a microstructured resin film or medium 645, which is available within the scope of this disclosure, is shown. Within the available scope, a microstructured lens can then be produced by injection molding using the microstructured first mold insert 635 on a first mold side (front side, concave side) and a glass protruding insert on a second mold side 630 (rear side). In a first step, the first mold insert 635 can be coupled to a second mold insert 640 in the mold to form a cavity. In a second step, a polymer melt (such as polycarbonate) can be injected into the cavity. In a third step, if the coupling was not fully completed in the first step, the first mold insert 635 and the second mold insert 640 can be fully coupled. In a fourth step, the mold can be opened after the polymer melt has sufficiently cooled, and the lens including the microstructured surface can be removed.
[0089] Within the available scope, a master mold 610 can be used to form an impression 615, and the impression 615 can be used to directly modify the surface of the finished lens. In a first step, the master mold 610 can be arranged in a container or have a gasket 605 formed around the master mold 610. In a second step, material (such as PDMS) for the impression 615 can be poured onto the master mold 610. Subsequently, for a master mold 610 arranged in a container, the hardened PDMS can be removed as a large sheet conforming to the shape of the container, and the desired area for the impression 615 can be cut or shaped from the large PDMS sheet. For a master mold 610 with the formed gasket 605, the PDMS impression 615 can be peeled off from the surface of the master mold 610. In a third step, the PDMS impression 615 can be pressed into a hard coating medium on a substrate (e.g., a lens) to imprint the impression 615 onto the hard coating medium on the substrate. For example, a droplet of hard coating medium solution can be dropped onto the surface of the lens, and a PDMS mold 615 can then be arranged on the droplet of hard coating medium to ensure that all features of the PDMS mold 615 are fully filled with the hard coating medium solution. In the fourth step, the hard coating medium can be polymerized, for example by UV photopolymerization, to solidify the features imparted by the mold 615. Notably, the PDMS is UV transparent, and the PDMS mold 615 can remain pressed into the surface of the lens. In the fifth step, the PDMS mold 615 can be delaminated or separated from the surface of the lens and the now polymerized and cured hard coating medium, which has microstructures formed therein based on a complementary pattern of the mold 615. In the sixth step, the lens with the microstructured hard coating medium formed thereon can be finished by various manufacturing methods to form the desired finished lens shape, thickness, formulation, and coatings, etc. Additional coatings may include, for example, anti-reflective coatings and anti-fouling coatings. Notably, the additional methods described herein can prevent the mold 615 and molding material from being exposed to the potentially high-temperature environment of injection molding. Conversely, lower-temperature polymerization can be achieved through UV light exposure.
[0090] Within the scope of applicability, the first mold insert 635 having a microstructured resin film or medium 645 can be used for injection molding as described, or for casting processes to produce a desired lens. That is, similar to the method of forming a gasket 605 to create an impression 615, a similar process can be performed using the first mold insert 635 having a microstructured resin film or medium 645 to cast a desired lens. Furthermore, the injection-molded or cast lens can be a semi-finished or finished lens. Additionally, within the scope of applicability, the molded or cast part can simply be a film or wafer substrate. Within the scope of applicability, the curvature of the impression 615 and the first mold insert 635 can be spherical, aspherical, concave, convex, planar, or progressive. Although the impression 615 described and shown in the accompanying drawings is shown as having the same area as the first mold insert 635, it is understood that the area of the impression 615 can be larger or smaller than the surface area of the first mold insert 635.
[0091] Within the limits of availability, the microstructured resin film or medium 645 can be transferred from the first mold insert 635 to the lens during molding. The injected polymer melt can then encapsulate the microstructured resin film or medium 645 and retain it on the surface of the lens.
[0092] Within the available scope, lens formation may include further adjustments to the formed lens based on the metrological results of the lens formed after the first cycle. That is, for example, after injection molding, the mold may be opened to remove the molded lens. Since the master mold 610 may be flat and the finished lens may be curved, some adjustments may be needed to compensate for deformations of the multiple microstructures 690 that may be introduced by the mismatch between the mold 615 and the finished lens. For example, the resulting microstructures on the curved lens may differ from those on the (flat) master mold 610 in terms of x-axis and y-axis position, shape, and depth or height along the z-axis (i.e., orthogonal to the plane of the lens surface). Shrinkage of the injected polymer, mold material, or resin imprinted on the mold insert surface may, for example, reduce the depth or height of the microstructure and result in changes in optical power or redistribution of optical energy in the diffraction order. Thus, the thickness of the molded lens can be determined, and when the thickness (or any other dimension) of the molded lens is determined to be below a predetermined threshold, the molded lens can be reinserted into the cavity for a second cycle. That is, the polymer melt can be re-injected into the cavity containing the molded lens. Due to various factors, including, for example, polymer shrinkage / contraction during cooling, the thickness (or any other dimension) of the molded lens after the first cycle may be less than expected. Therefore, the second cycle can reduce the variance introduced by such example factors. Additionally, compensation can be incorporated into the dimensions of the master mold 610 (e.g., during the photolithography fabrication of the master mold 610) and the subsequent impression mold 615 for the microstructure height.
[0093] Figure 13B Exemplary cross-sectional profiles of two microstructures available within the scope of this disclosure are shown. As illustrated, the “ΔZ” designation indicates the difference between the expected theoretical microstructure curve and the obtained microstructure curve, where the lower of the two curves is the obtained microstructure curve, which exhibits contraction and is therefore less deep or high. This difference can therefore be considered and compensated for during the fabrication of the master mold 610. Alternatively, the hard coating medium solution can be changed to use a hard coating medium solution with a higher refractive index to compensate, such that the order energy will be adjusted accordingly based on the obtained microstructure. For example, when the 0th order energy is lowered, the +1st order energy will be increased.
[0094] Example
[0095] Examples 1 to 5 Figure 14Differential scanning calorimetry (DSC) plots for various examples are shown. DSC plots for SU-8 examples were performed to understand how the chemistry of UV-cured SU-8 behaves at elevated temperatures. This data provides insights into the possible post-exposure bake (PEB) temperatures that would allow the SU-8 layer to be stable during the elevated temperatures experienced during injection molding of myopia control lenses. For example, the mold used for injection molding can be set at a temperature lower than the Tg of polycarbonate, but the insert surface can reach higher temperatures when the melt first contacts the insert surface.
[0096]
[0097] Table 1 - Example Compositions
[0098] Epoxy groups cannot be fully cured by UV exposure alone and require additional thermal heating for more complete conversion. For example, these examples show a clear trend in the reaction peak in DSC data, exhibiting an onset exothermic temperature that shifts higher with increasing PEB temperature. Example 1 shows that the SU-8 layer in PEB at 110°C will be stable at temperatures up to 150°C and will still contain some unreacted epoxy groups. A PEB temperature of 200°C, as shown in Example 5, will provide the most stable conditions because no residual exothermic temperature indicates that all epoxy groups have reacted. Furthermore, the onset exothermic peak at 130°C for two hours isothermally ...
[0099] Examples 6 through 12 – Constructing flat silicon wafers using the techniques described in this paper to evaluate replication quality.
[0100] Step 1: Using a spin coater set to 1500 RPM, coat a flat silicon wafer with SU-8 coating material obtained from Kayaku Advanced Materials.
[0101] Step 2: The wafer is softened in an oven at 110°C for 2 hours to evaporate all solvents and obtain pure SU-8 with a thickness of 20 μm.
[0102] Step 3: A flat PDMS impression, cast from a NiP steel microstructured master mold, was pressed into the SU-8 layer under various temperatures and pressures. The inverted structures on the impression were characterized by microscopy and were found to have the same dimensions as the microstructures on the master mold. These structures are quasi-spherical with a base diameter of 1.17 mm and a height of 7.0 μm (see [link to original text]). Figure 15 ).
[0103] Step 4: Lower the ambient temperature to below 30°C and maintain the mold under a predetermined pressure until the temperature reaches at least 30°C.
[0104] Step 5: Carefully peel the impression from the surface of the SU-8 resin film.
[0105] Step 6: Expose the wafer / SU-8 to UV light for 2 minutes (alternatively, UV curing can be performed before step 5).
[0106] Step 7: First, observe the replicated structure on the wafer with your eyes, and if it is visible to the naked eye, analyze it later with a microscope.
[0107]
[0108] Table 2
[0109] Figure 15 Microscopic images and microstructural outlines of inverted microstructures obtained on PDMS impressions used in Examples 5 through 11 are shown. These were taken using a Keyence VK-X200 series microscope at 1000x magnification.
[0110] Figure 16 An optical image of the replicated microstructure from the SU-8 layer of Example 9 is shown.
[0111] Examples 13, 14 and 15 – Concave glass inserts were constructed using techniques as described herein to evaluate replication quality and durability during injection molding.
[0112] These steps are similar to those described for Examples 6-12, with the following modifications: (1) the NiP steel microstructure master mold has a concave base arc of 3.25 diopter and contains smaller microstructures (base diameter = 1.17 mm; depth = 1.4 μm); (2) replicating from the NiP master mold as follows Figure 17 The PDMS impression shown; (3) The SU-8 layer was applied by brush rather than spin coating because no suitable spin coater was available for this heavy-duty insert. For Examples 13 and 14, the approximate SU-8 thickness after soft baking was 5 μm at the thinnest point and about 20 μm in the thicker areas. Example 15 had a more consistent SU-8 thickness between 20 and 100 μm; (4) The stamping temperature and pressure for Examples 13 and 14 were 115 °C and 3.3 psi, respectively; and the stamping temperature and pressure for Example 15 were 115 °C and 4.3 psi, respectively; and (5) For Example 13, the structured SU-8 / insert was post-baked at 130 °C for 3 hours, for Example 14, at 150 °C for 3 hours, and for Example 15, at 175 °C for 3 hours.
[0113]
[0114] Table 3 - Examples of Microscopic Examination
[0115] Figure 17 Microscopic images and microstructure profiles of the inverted microstructures obtained on PDMS impressions used in Examples 13, 14, and 15 are shown. These were taken using a Keyence VK-X200 series camera at 1000x magnification. Analysis of the results indicates good reproduction of Examples 13, 14, and 15. This suggests that PDMS impressions with a 20 μm SU-8 layer thickness are suitable for smaller structures up to 1.4 μm deep. PDMS has a low elastic modulus and is easily compressed. In the case of larger structures, more SU-8 material will need to be penetrated and pushed towards the periphery of the impression. The flow of SU-8 will become increasingly confined to the insert surface. More rigid impressions with an increased elastic modulus or a thicker SU-8 layer would be beneficial for spherical structures up to 7.0 μm deep.
[0116] Examples 13 and 14 demonstrate that the structure remains stable even at 150°C PEB, as the microstructural dimensions from the master mold to the PDMS impression to the SU-8 / insert replica remain essentially unchanged even after PEB. Injection molding tests are performed in repeated cycles. After each cycle, a part is produced, which is also referred to here as the injection part. For example, injection part 10 will be the 10th part of the 10th cycle. Example 15 gives the best results in terms of durability during injection molding. This is due to the increased SU-8 thickness and PEB temperature. The increased thickness is the primary reason, as the thickness at which delamination occurs appears to be limited, as evidenced by the absence of delamination in the areas of Examples 13 and 14 with higher thicknesses. Due to heat transfer from the melt, the expansion of SU-8 relative to glass at the SU-8 / glass interface will increase with decreasing thickness. Incorporating silica nanoparticles (GLM2060 low-stress, supplied by Gersteltec Engineering Solutions) into the SU-8 provides an optimal solution for increasing PEB temperature and minimizing thickness, for example, if delamination is likely to occur after injection molding 200.
[0117] Figure 18AMicrostructure optics results for measuring the optical power of each microstructure for lenses of Examples 15 and 16 are shown. Results for each ring of the microstructure pattern (such as a microlens array) are calculated. The design studied has a total of 11 rings. Each ring contains multiple microlenses positioned at a predetermined diameter from the optical center of the lens. Ring 1 can be closest to the optical center, and ring 11 can be furthest from the optical center; the optical power gradually decreases as the number of rings increases. The results for Example 15 (injection molded parts 10 and 200) are compared with those for Injection Mold 10 of Example 16. Example 16 was produced by injection molding the lens directly from a microstructured NiP steel master mold. The results show that the replicated structure of Example 15 is very stable during injection molding, with essentially no change in optical power from Injection Mold 10 to Injection Mold 200. The results for Example 15 differ slightly from those for rings 1 to 7 of Example 16, but are the same as those for rings 8 to 11. For a first attempt, the change is minimal and very close, and can be improved by optimizing stamping conditions or injection molding parameters (specifically, stamping material, stamping temperature and pressure distribution, SU-8 layer thickness consistency, mismatch between the stamp base arc and the insert base arc; and injection molding die temperature, speed, and pressure).
[0118] Figure 18B Microscopic images and microstructural profiles of a lens produced by Example 12, available within the scope of this disclosure, are shown. As illustrated, multiple inverted microstructures 190 are well replicated on the surface of the lens to produce multiple microstructures 195. Example 12 demonstrates that high-quality myopia control lenses with stable microstructural geometries can be produced by the method described herein. For example, a lens from the 100th injection unit can have the same structure as one from, for example, the 6th injection unit.
[0119] Example 16- Figure 19 This is an optical image of the master mold 610, which includes the microstructure. The microstructured molten silica planar master mold 610 was treated with O2 plasma and silane under vacuum for at least 6 hours, and then cleaned with alcohol. Adhesive tape was applied around the master mold 610 to form a gasket 605. UV-grade PDMS (KER4690 A+B) was prepared and degassed for the first time under vacuum.
[0120] Figure 20 This is a schematic diagram of a female mold 610 including PDMS filled in washer 605. Figure 21This is an optical image of the master mold 610, which includes PDMS filled in gasket 605. Uncured PDMS is then poured into gasket 605 along the surface of the flat master mold 610. In this example, 16g of PDMS is used to form a 2mm thick film. The PDMS is degassed again under vacuum to allow the viscous PDMS to fill multiple inverted microstructures 695. Curing of the PDMS is performed under a UV light source (e.g., a mercury lamp) for at least 5 minutes. Once fully cured, the PDMS is carefully pulled out, cured again, and stored as a mold 615 to prevent dust and other microparticles from entering.
[0121] Figure 22A It is an optical image of the first mold insert 635, which is partially machined. Figure 22B The first mold insert 635 has a finished surface. The first mold insert 635 is first rough-turned or medium-turned on a lathe, followed by (finer) diamond turning on a higher-precision lathe to form the desired radius of curvature and low surface roughness of the first mold insert 635. Subsequently, the first mold insert 624 is treated with O2 plasma and coated by spin coating with the main reagents for the glass substrate according to Table 4.
[0122]
[0123] Table 4 - Coating conditions for main reagents
[0124] After baking and cooling, the hybrid resin (ORMOSTAMP from Micro Resist Technology) was spin-coated according to Table 5. The thickness of the resin film or dielectric 645 was determined to be between 1 and 10 μm.
[0125] Coating material OrmoStamp film thickness 10±1μm Rotation speed 3000RPM Rotation time 30s Rotational acceleration 1000 RPM / s Pre-baking (heating plate) temperature 80℃ Pre-baking (heating plate) time 2min Exposure dose (at 365nm) <![CDATA[1000mJ / cm 2 ]]> Post-baking (heating plate) temperature 130℃ Post-baking (heating plate) time 10-30 min OrmoDev (developer) 60-180s
[0126] Table 5 - Resin Coating Conditions
[0127] Figure 23 This is an optical image of the holding device for the impression 625. The PDMS impression 615 is arranged and fixed to... Figure 23The holding device shown is similar to those used in experimental lamination apparatuses. Notably, a vacuum can be used to hold the impression 615 to the holding device. Notably, the impression 615 may have a slight curvature such that the center of the impression 615 contacts the first mold insert 635 first (the edge last). The impression 615 can be pressed into the first mold insert 635, which includes a resin film or medium 645. For example, the impression 615 can be pressed into the first mold insert 635 for a predetermined time length, such as 10 seconds, 1 minute, 5 minutes, 10 minutes, 15 minutes, 20 minutes, or between 5 seconds and 30 minutes, and at various speeds from 0.01 mm / s to 10 mm / s, for example, for a predetermined time length.
[0128] Figure 24 This is an optical image of the impression 615 pressed into the resin film or medium 645 during curing. While the impression 615 is fully pressed into the first mold insert 635 and the resin film or medium 645, the UV light source can be activated for, for example, 1 minute, 2 minutes, 5 minutes, more than 30 seconds, or preferably 90 seconds. After irradiation, the impression 615 is removed from the resin film or medium 645. The first mold insert 635, comprising the microstructured resin film or medium 645, is then post-cured.
[0129] Figure 25 It is an optical image of a first mold insert 635 including a microstructured resin film or medium 645. At least 100 lenses are then injection molded using the first mold insert 635 including the microstructured resin film or medium 645. Figure 26 This is an optical image of the first mold insert 635 with a partially delaminated microstructured resin film or medium 645. Even after more than 100 lenses, only slight delamination of the microstructured resin film or medium 645 is observed.
[0130] It is worth noting that after measuring the replicated microstructure in the lens and determining the necessary adjustments, further improvements can be made to the precision of the resin film or medium 645 used for replication via injection molding. For example, higher aspect ratios, different aspect ratios, different curvatures, etc.
[0131] Advantageously, the above method can be used to imprint other materials. For example... Figure 27A As shown, Figure 27A This is an optical image of a 40nm thick copper layer deposited on a glass mold insert. The glass mold insert can be planar, convex, or concave and is used for nickel stamping. Figure 27B As shown, Figure 27B It is an optical image of an MR8 substrate including an imprinted hard coating. For example... Figure 27C As shown, Figure 27C It is an optical image of the imprinted phenolic film.
[0132] Figure 28 This is an exemplary flowchart of a method 1900 for fabricating a microstructured insert that is available within the scope of this disclosure. In step 1910, an impression is formed. In step 1920, the impression is pressed into a resin film or medium 645 on the surface of a first mold insert 635. In step 1930, a lens is fabricated by injection molding using the first mold insert 635 having a microstructured resin film or medium 645 formed on the surface of the first mold insert 635.
[0133] In the foregoing description, specific details, such as the particular geometry of the processing system and the description of the various components and processes used therein, have been set forth. However, it should be understood that the techniques described herein can be practiced in other embodiments departing from these specific details, and such details are for illustrative purposes rather than limiting. Embodiments disclosed herein have been described with reference to the accompanying drawings. Similarly, specific figures, materials, and configurations have been set forth for illustrative purposes to provide a thorough understanding. However, embodiments can be practiced without such specific details. Components having substantially the same functional structure are denoted by the same reference numerals, and therefore any redundant description may be omitted.
[0134] Various techniques have been described as multiple discrete operations to aid in understanding the various embodiments. The order of the descriptions should not be construed as implying that these operations necessarily depend on a specific order. In fact, these operations do not need to be performed in the order presented. Unless otherwise expressly indicated, the described operations may be performed in an order different from that specifically described. Various additional operations may be performed and / or the described operations may be omitted.
[0135] Those skilled in the art will also understand that many changes can be made to the operation of the techniques described above while still achieving the same objectives of this disclosure. Such changes are intended to be covered by the scope of this disclosure. Thus, the above description of the embodiments is not intended to be limiting. Rather, any limitations on the embodiments are set forth in the following claims.
[0136] The embodiments disclosed herein may also be described as shown in the following parentheses.
[0137] (1) A method of forming a mold insert, the method comprising: forming an impression (615) having a surface of the impression (615) including a plurality of inverted microstructures (695) formed thereon; and pressing the impression (615) into a membrane or medium (645) disposed on a surface of a first mold insert (635) to form a microstructured membrane (645), the microstructured membrane (645) including a plurality of microstructures (690) formed on the surface of the microstructured membrane (645) based on the plurality of inverted microstructures (695), the plurality of microstructures (690) being complementary to the plurality of inverted microstructures (695).
[0138] (2) The method as described in (1), wherein the method further comprises covering the surface of the first mold insert (635) with resin to form the medium (645); and soft baking the first mold insert (635) covered with the medium (645) of the resin.
[0139] (3) The method of any one of (1) or (2), the method further comprising curing the medium (645); and baking the medium (645) to a thickness between 0.1 μm and 300 μm.
[0140] (4) The method of any one of (1) to (3), the method further comprising: arranging the first mold insert (635) having the microstructured membrane (645) formed thereon in a molding apparatus including a second mold insert (640); the first mold insert (635) having the microstructured membrane (645) formed thereon and the second mold insert (640) forming a cavity; closing the first mold insert (635) having the microstructured membrane (645) formed thereon and the second mold insert (640); and injecting a polymer into the cavity.
[0141] (5) The method as described in (1), wherein the impression is pressed into the medium to obtain the difference between the base arc of the impression (615) and the base arc of the first mold insert (635) within ±0.5 diopters.
[0142] (6) The method of any one of (1) to (5), wherein covering the surface of the first mold insert (635) further comprises treating the surface of the first mold insert (635) with plasma before covering the surface of the first mold insert (635) with the resin.
[0143] (7) The method of any one of (1) to (6), wherein pressing the impression (615) into the medium (645) further comprises attaching the impression (615) to a first fixing device (650); attaching the first mold insert (635) having the microstructured membrane (645) formed thereon to a second fixing device (655), the first fixing device (650) and the second fixing device (655) being configured to engage and align the impression (615) with the first mold insert (635) and the medium (645); and engaging the first fixing device (650) having the attached impression (615) and the second fixing device (655) having the attached first mold insert (635).
[0144] (8) The method of any one of (1) to (7), the method further comprising decoupling the impression (615) from the microstructured membrane (645) at a temperature of less than 50°C.
[0145] (9) The method of any one of (2) to (8), wherein the resin is SU-8 dispersed in a solvent with a total solvent content ranging from 0% to 50%.
[0146] (10) The method of any one of (2) to (9), wherein the resin comprises oxide nanoparticles.
[0147] (11) The method of any one of (1) to (10), wherein forming the mold (615) further comprises coating, casting, or injection molding polymer from the surface of the master mold; curing the coated or cast polymer or cooling the injection molding polymer to form the mold (615); and removing the mold (615) from the master mold.
[0148] (12) The method of (11), wherein the material of the coated or cast polymer includes polydimethylsiloxane (PDMS), fluorinated ethylene propylene (FEP), or polytetrafluoroethylene (PTFE), and the injection-molded polymer includes cyclic olefin copolymers, polystyrene, polymethyl methacrylate, or polymethylpentene.
[0149] (13) The method of any one of (1) to (12), wherein forming the impression (615) further comprises turning the plurality of inverted microstructures (695) diamond onto a metal or polymer and covering the surface of the impression (615) with a nanolayer.
[0150] (14) A molding apparatus comprising a mold, the mold including a first mold insert (635) and a second mold insert (640), the first mold insert (635) including a microstructured film (645) disposed on a surface of the first mold insert (635), the microstructured film (645) including a plurality of microstructures (690) formed thereon, wherein the material of the first mold insert (635) is glass or metal, and the material of the microstructured film (645) is resin, preferably a resin including epoxy functional groups or SU-8.
[0151] (15) The apparatus as described in (14) further includes processing circuitry configured to connect the first mold insert (635) and the second mold insert (640) having the microstructured membrane (645) disposed thereon to form a cavity; close the first mold insert (635) and the second mold insert (640) having the microstructured membrane (645) formed thereon; and inject a polymer into the cavity.
[0152] (16) The method as described in (4), wherein the injected polymer melt is polycarbonate.
[0153] (17) The method as described in (4), the method further comprising opening the first mold insert (635) and the second mold insert (640) having the microstructured film (645) formed thereon to remove the molded lens; determining the thickness of the molded lens; and when the thickness of the molded lens is determined to be below a predetermined threshold, inserting the molded lens into the cavity and re-injecting the polymer melt into the cavity including the molded lens.
[0154] (18) The method of any one of (2) to (13), wherein the material of the first mold insert (635) is glass, metal, steel, aluminum, metal alloy or composite material.
[0155] (19) The method as described in (5), wherein the molded lens is a multilayer film, a semi-finished lens, a finished lens, or a wafer.
[0156] (20) The method of any one of (2) to (13), wherein the area of the impression (615) is greater than the surface of the first mold insert (635).
[0157] (21) The method of any one of (2) to (13), wherein the area of the impression (615) is smaller than the surface of the first mold insert (635).
[0158] (22) The method of any one of (1) or (2), wherein the thickness of the medium (645) is between 0.1 μm and 500 μm, or 0.5 μm and 400 μm, or 0.75 μm and 350 μm.
[0159] (23) The method of any one of (2) to (13), wherein the medium (645) is coated on the auxiliary component and the auxiliary component is assembled on the first mold insert (635).
[0160] (24) The method of any one of (2) to (13), wherein the impression (615) is formed by machining or photolithography.
[0161] (25) The method as described in (3), the method further comprising carving the medium (645) before or after post-baking.
[0162] (26) The method as described in (25), wherein engraving the medium (645) further includes engraving position marks, codes, or design references in the medium (645).
[0163] (27) The method of any one of (1) to (13), wherein the material of the impression (615) has an elastic modulus greater than 0.5 MPa, and pressing the impression (615) into the medium (645) further comprises pressing the impression (615) into the medium (645) at a temperature between 10°C and 250°C, or 15°C and 200°C, or 15°C and 180°C and at a pressure less than 20,000 psi, or less than 15,000 psi, or less than 10,000 psi, or between 1 psi and 10,000 psi.
[0164] (28) An optical lens manufactured using the method described in (4).
[0165] (29) The method as described in (28), wherein the surface curvature of the optical lens is spherical, aspherical, concave, convex, flat, or progressive.
[0166] (30) The method of any one of (2) to (13), wherein the surface of the first mold insert (635) is covered with the resin to form the medium (645) by spin coating, spraying, scraping, dipping, molding or lamination.
[0167] (31) The method of any one of (1) to (13), wherein the impression is formed by machining, diamond turning or photolithography.
[0168] (32) A method of forming a lens, the method comprising: forming an impression (615) having a surface including a plurality of inverted microstructures (695) formed thereon; and pressing the impression (615) into a film or medium (645) disposed on the surface of the lens to form a microstructured film (645), the microstructured film (645) including a plurality of microstructures (690) formed on the surface of the microstructured film (645) based on the plurality of inverted microstructures (695), the plurality of microstructures (690) being complementary to the plurality of inverted microstructures (695).
Claims
1. A method for forming a mold insert, comprising: An impression (615) is formed, the surface of which includes a plurality of inverted microstructures (690) formed thereon. as well as The impression (615) is pressed into a medium (645) disposed on the surface of a first mold insert (635) to form a microstructured film, the microstructured film comprising a plurality of microstructures (695) formed on the surface of the microstructured film based on the plurality of inverted microstructures, the plurality of microstructures (695) being complementary to the plurality of inverted microstructures (690) formed on the impression (615), and The impression (615) is disassembled to obtain a first mold insert having the microstructured membrane formed thereon. The method further includes: The medium (645) is formed by covering at least a portion of the surface of the first mold insert (635) with resin, wherein the resin is an epoxy resin having an octafunctional epoxy molecule; and The first mold insert (635) covered with the medium (645) is soft-baked.
2. The method of claim 1, wherein the method further comprises To cure the medium (645); and The medium (645) is then baked to a thickness between 0.1 µm and 300 µm.
3. The method as described in claim 1 or 2, wherein, The impression (615) is pressed into the medium (645) to obtain the difference between the base arc of the impression (615) and the base arc of the first mold insert (635) within ± 0.5 diopters.
4. The method as described in claim 1 or 2, wherein, The surface covering the first mold insert (635) further includes treating the surface of the first mold insert (635) with plasma before covering the surface of the first mold insert (635) with the medium (645).
5. The method as described in claim 1 or 2, wherein, Pressing the impression (615) into the medium (645) further includes The impression (615) is attached to the first fixing device (650). The first mold insert (635) having the microstructured membrane formed thereon is attached to the second fixing device (655), the first fixing device (650) and the second fixing device (655) being configured to connect and align the impression (615) with the first mold insert (635) and the medium (645); as well as The first fixing device (650) having the attached mold (615) and the second fixing device (655) having the attached first mold insert (635) are connected.
6. The method of claim 1 or 2, further comprising uncoupling the impression (615) from the microstructured membrane at a temperature less than 50°C.
7. The method as described in claim 1 or 2, wherein, The material of the impression (615) has an elastic modulus greater than 0.5 MPa, and pressing the impression (615) into the medium (645) further includes pressing the impression (615) into the medium (645) at a temperature between 15°C and 180°C and a pressure less than 10,000 psi.
8. The method as claimed in claim 1 or 2, wherein, The resin comprises oxide nanoparticles.
9. The method as claimed in claim 1 or 2, wherein, Forming the impression (615) further includes Polymers are coated, cast, or injection molded from the surface of the master mold (610); Curing the coated or cast polymer or cooling the injection-molded polymer to form the mold (615); and Remove the impression (615) from the master mold (610).
10. The method of claim 9, wherein, The materials of the coated or cast polymer include polydimethylsiloxane (PDMS), fluorinated ethylene propylene (FEP), or polytetrafluoroethylene (PTFE), and the injection-molded polymer includes cyclic olefin copolymers, polystyrene, polymethyl methacrylate, or polymethylpentene.
11. The method as claimed in claim 1 or 2, wherein, Forming the impression (615) further includes The plurality of inverted microstructures (690) are diamond-machined onto a metal or polymer and the surface of the impression (615) is covered with a nanolayer.
12. A molding apparatus comprising: A mold, the mold comprising at least a first mold insert (635), the first mold insert (635) having a microstructured membrane (645) disposed thereon, the microstructured membrane (645) comprising a plurality of microstructures (695) formed thereon, wherein The first mold insert (635) is made of glass or metal, and the microstructured film (645) is made of epoxy resin, which is an epoxy resin with octafunctional epoxy molecules.
13. The molding apparatus of claim 12, further comprising processing circuitry configured to... The first mold insert and the second mold insert having the microstructured membrane disposed thereon are connected to form a cavity; Close the first mold insert and the second mold insert having the microstructured membrane formed thereon; as well as The polymer is injected into the cavity.
14. A method for forming a mold insert, comprising: The method according to any one of claims 1 to 11 forms a first mold insert (635) having a microstructured membrane (645) formed thereon. A first mold insert (635) having the microstructured membrane (645) formed thereon is arranged in a molding apparatus including a second mold insert (640), the first mold insert (635) having the microstructured membrane (645) formed thereon and the second mold insert (640) forming a cavity; The first mold insert (635) and the second mold insert (640) having the microstructured membrane (645) formed thereon are closed; as well as The polymer is injected into the cavity.
Citation Information
Patent Citations
Lens element
US20210109379A1
Resin mold for nanoimprinting and manufacturing method thereof
CN103068556A
Method and apparatus for making an ophthalmic lens containing a Fresnel-surface
EP2594392A2